| Category | Polymer , Thermoplastic , Nylon |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® RS |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® RS LC1010 NC010 Nylon 1010
(Unverified Data**).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.05 g/cc | 0.0379 lb/in³ | DAM; ISO 1183 |
| Moisture Absorption | 1.10 % @Thickness 2.00 mm |
1.10 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Viscosity | 230000 cP @Temperature 250 °C |
230000 cP @Temperature 482 °F |
DAM; @ 1000 sec-1; ISO 11443 |
| Linear Mold Shrinkage, Flow | 0.014 cm/cm | 0.014 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.010 cm/cm | 0.010 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Stress | 0.340 MPa @Strain 0.230 %, Temperature 150 °C |
49.3 psi @Strain 0.230 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 |
| 1.01 MPa @Strain 0.250 %, Temperature 90.0 °C |
146 psi @Strain 0.250 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 1.72 MPa @Strain 1.02 %, Temperature 150 °C |
249 psi @Strain 1.02 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 1.82 MPa @Strain 0.250 %, Temperature 40.0 °C |
264 psi @Strain 0.250 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 3.18 MPa @Strain 0.150 %, Temperature 0.000 °C |
461 psi @Strain 0.150 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 4.39 MPa @Strain 0.210 %, Temperature 0.000 °C |
637 psi @Strain 0.210 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 4.83 MPa @Strain 0.250 %, Temperature 23.0 °C |
701 psi @Strain 0.250 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 5.13 MPa @Strain 0.200 %, Temperature -40.0 °C |
744 psi @Strain 0.200 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 5.30 MPa @Strain 0.270 %, Temperature 0.000 °C |
769 psi @Strain 0.270 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 5.34 MPa @Strain 4.52 %, Temperature 150 °C |
775 psi @Strain 4.52 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 6.68 MPa @Strain 1.93 %, Temperature 90.0 °C |
969 psi @Strain 1.93 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 6.72 MPa @Strain 6.01 %, Temperature 150 °C |
975 psi @Strain 6.01 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 7.98 MPa @Strain 9.99 %, Temperature 150 °C |
1160 psi @Strain 9.99 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 9.18 MPa @Strain 0.390 %, Temperature -40.0 °C |
1330 psi @Strain 0.390 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 9.34 MPa @Strain 0.690 %, Temperature 23.0 °C |
1350 psi @Strain 0.690 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 9.63 MPa @Strain 15.15 %, Temperature 150 °C |
1400 psi @Strain 15.15 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 9.82 MPa @Strain 19.73 %, Temperature 150 °C |
1420 psi @Strain 19.73 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 10.08 MPa @Strain 1.19 %, Temperature 40.0 °C |
1462 psi @Strain 1.19 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 10.38 MPa @Strain 20.97 %, Temperature 150 °C |
1505 psi @Strain 20.97 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 12.03 MPa @Strain 134.97 %, Temperature 150 °C |
1745 psi @Strain 134.97 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 12.38 MPa @Strain 143.05 %, Temperature 150 °C |
1796 psi @Strain 143.05 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 12.59 MPa @Strain 4.43 %, Temperature 90.0 °C |
1826 psi @Strain 4.43 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 14.72 MPa @Strain 6.46 %, Temperature 90.0 °C |
2135 psi @Strain 6.46 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 16.91 MPa @Strain 0.840 %, Temperature 0.000 °C |
2453 psi @Strain 0.840 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 17.22 MPa @Strain 9.14 %, Temperature 90.0 °C |
2498 psi @Strain 9.14 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 18.84 MPa @Strain 13.03 %, Temperature 90.0 °C |
2733 psi @Strain 13.03 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 20.01 MPa @Strain 17.69 %, Temperature 90.0 °C |
2902 psi @Strain 17.69 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 21.21 MPa @Strain 29.48 %, Temperature 90.0 °C |
3076 psi @Strain 29.48 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 22.97 MPa @Strain 123.75 %, Temperature 90.0 °C |
3332 psi @Strain 123.75 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 23.66 MPa @Strain 124.65 %, Temperature 90.0 °C |
3432 psi @Strain 124.65 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 26.25 MPa @Strain 5.74 %, Temperature 40.0 °C |
3807 psi @Strain 5.74 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 28.95 MPa @Strain 7.45 %, Temperature 40.0 °C |
4199 psi @Strain 7.45 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 30.08 MPa @Strain 2.64 %, Temperature 23.0 °C |
4363 psi @Strain 2.64 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 32.38 MPa @Strain 12.17 %, Temperature 40.0 °C |
4696 psi @Strain 12.17 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 33.88 MPa @Strain 1.73 %, Temperature 0.000 °C |
4914 psi @Strain 1.73 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 35.84 MPa @Strain 37.96 %, Temperature 40.0 °C |
5198 psi @Strain 37.96 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 35.9 MPa @Strain 33.83 %, Temperature 40.0 °C |
5210 psi @Strain 33.83 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 36.26 MPa @Strain 123.61 %, Temperature 40.0 °C |
5259 psi @Strain 123.61 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 36.53 MPa @Strain 22.75 %, Temperature 40.0 °C |
5298 psi @Strain 22.75 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 37.33 MPa @Strain 4.84 %, Temperature 23.0 °C |
5414 psi @Strain 4.84 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 42.04 MPa @Strain 8.77 %, Temperature 23.0 °C |
6097 psi @Strain 8.77 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 45.71 MPa @Strain 2.12 %, Temperature -40.0 °C |
6630 psi @Strain 2.12 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 46.79 MPa @Strain 20.9 %, Temperature 23.0 °C |
6786 psi @Strain 20.9 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 47.6 MPa @Strain 2.65 %, Temperature 0.000 °C |
6900 psi @Strain 2.65 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 48.23 MPa @Strain 3.40 %, Temperature 23.0 °C |
6995 psi @Strain 3.40 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 49.13 MPa @Strain 2.35 %, Temperature -40.0 °C |
7126 psi @Strain 2.35 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 51.6 MPa @Strain 3.22 %, Temperature 0.000 °C |
7480 psi @Strain 3.22 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 59.13 MPa @Strain 5.77 %, Temperature 0.000 °C |
8576 psi @Strain 5.77 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 62.07 MPa @Strain 16.38 %, Temperature 0.000 °C |
9003 psi @Strain 16.38 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 67.4 MPa @Strain 3.69 %, Temperature -40.0 °C |
9780 psi @Strain 3.69 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 71.74 MPa @Strain 4.04 %, Temperature -40.0 °C |
10410 psi @Strain 4.04 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 76.32 MPa @Strain 4.75 %, Temperature -40.0 °C |
11070 psi @Strain 4.75 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 83.07 MPa @Strain 5.65 %, Temperature -40.0 °C |
12050 psi @Strain 5.65 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 89.17 MPa @Strain 11.02 %, Temperature -40.0 °C |
12930 psi @Strain 11.02 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| Tensile Strength, Yield | 43.0 MPa | 6240 psi | 50%RH; ISO 527-1/-2 |
| 52.0 MPa | 7540 psi | DAM; ISO 527-1/-2 | |
| Elongation at Break | >= 50 % | >= 50 % | DAM; Nominal; ISO 527-1/-2 |
| >= 50 % | >= 50 % | 50%RH; Nominal; ISO 527-1/-2 | |
| Elongation at Yield | 4.5 % | 4.5 % | DAM; ISO 527-1/-2 |
| 30 % | 30 % | 50%RH; ISO 527-1/-2 | |
| Tensile Modulus | 0.950 GPa | 138 ksi | 50%RH; ISO 527-1/-2 |