| Category | Polymer , Thermoplastic , Nylon , Nylon 610 |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® RS |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® RS 30G30L NC010 Nylon 610.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.16 g/cc | 0.0419 lb/in³ | |
| 1.31 g/cc | 0.0473 lb/in³ | DAM; ISO 1183 | |
| Moisture Absorption | 1.20 % @Thickness 2.00 mm |
1.20 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Viscosity | 93100 cP @Shear Rate 5000 1/s, Temperature 280 °C |
93100 cP @Shear Rate 5000 1/s, Temperature 536 °F |
ISO 11403-1 -2 |
| 123000 cP @Shear Rate 5000 1/s, Temperature 260 °C |
123000 cP @Shear Rate 5000 1/s, Temperature 500 °F |
ISO 11403-1 -2 | |
| 135400 cP @Shear Rate 5000 1/s, Temperature 250 °C |
135400 cP @Shear Rate 5000 1/s, Temperature 482 °F |
ISO 11403-1 -2 | |
| 305600 cP @Shear Rate 500 1/s, Temperature 280 °C |
305600 cP @Shear Rate 500 1/s, Temperature 536 °F |
ISO 11403-1 -2 | |
| 420900 cP @Shear Rate 500 1/s, Temperature 260 °C |
420900 cP @Shear Rate 500 1/s, Temperature 500 °F |
ISO 11403-1 -2 | |
| 491800 cP @Shear Rate 500 1/s, Temperature 250 °C |
491800 cP @Shear Rate 500 1/s, Temperature 482 °F |
ISO 11403-1 -2 | |
| Linear Mold Shrinkage, Flow | 0.0020 cm/cm | 0.0020 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.0070 cm/cm | 0.0070 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 130 MPa | 18900 psi | 50%RH; ISO 527-1/-2 |
| 160 MPa | 23200 psi | DAM; ISO 527-1/-2 | |
| Tensile Stress | 7.36 MPa @Strain 0.230 %, Temperature 150 °C |
1070 psi @Strain 0.230 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 |
| 8.44 MPa @Strain 0.180 %, Temperature 90.0 °C |
1220 psi @Strain 0.180 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 10.17 MPa @Strain 0.310 %, Temperature 150 °C |
1475 psi @Strain 0.310 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 10.94 MPa @Strain 0.190 %, Temperature 40.0 °C |
1587 psi @Strain 0.190 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 16.49 MPa @Strain 0.220 %, Temperature 23.0 °C |
2392 psi @Strain 0.220 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 18.68 MPa @Strain 0.210 %, Temperature 0.000 °C |
2709 psi @Strain 0.210 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 19.66 MPa @Strain 0.240 %, Temperature 40.0 °C |
2851 psi @Strain 0.240 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 19.79 MPa @Strain 0.460 %, Temperature 90.0 °C |
2870 psi @Strain 0.460 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 20.88 MPa @Strain 0.230 %, Temperature 23.0 °C |
3028 psi @Strain 0.230 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 22.51 MPa @Strain 0.230 %, Temperature 0.000 °C |
3265 psi @Strain 0.230 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 25.2 MPa @Strain 0.250 %, Temperature -40.0 °C |
3650 psi @Strain 0.250 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 28.2 MPa @Strain 1.23 %, Temperature 150 °C |
4090 psi @Strain 1.23 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 30.63 MPa @Strain 0.860 %, Temperature 90.0 °C |
4443 psi @Strain 0.860 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 39.8 MPa @Strain 0.840 %, Temperature 40.0 °C |
5770 psi @Strain 0.840 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 40.34 MPa @Strain 0.370 %, Temperature -40.0 °C |
5851 psi @Strain 0.370 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 40.58 MPa @Strain 2.48 %, Temperature 150 °C |
5886 psi @Strain 2.48 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 41.59 MPa @Strain 2.31 %, Temperature 150 °C |
6032 psi @Strain 2.31 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 48.43 MPa @Strain 3.85 %, Temperature 150 °C |
7024 psi @Strain 3.85 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 49.23 MPa @Strain 1.78 %, Temperature 90.0 °C |
7140 psi @Strain 1.78 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 49.24 MPa @Strain 0.570 %, Temperature 0.000 °C |
7142 psi @Strain 0.570 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 49.35 MPa @Strain 0.780 %, Temperature 23.0 °C |
7158 psi @Strain 0.780 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 53.28 MPa @Strain 1.82 %, Temperature 90.0 °C |
7728 psi @Strain 1.82 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 55.92 MPa @Strain 4.50 %, Temperature 150 °C |
8111 psi @Strain 4.50 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 62.58 MPa @Strain 0.730 %, Temperature 23.0 °C |
9076 psi @Strain 0.730 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 62.93 MPa @Strain 0.850 %, Temperature 40.0 °C |
9127 psi @Strain 0.850 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 63.21 MPa @Strain 2.95 %, Temperature 90.0 °C |
9168 psi @Strain 2.95 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 64.45 MPa @Strain 1.63 %, Temperature 40.0 °C |
9348 psi @Strain 1.63 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 64.96 MPa @Strain 6.96 %, Temperature 150 °C |
9422 psi @Strain 6.96 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 65.29 MPa @Strain 0.730 %, Temperature 0.000 °C |
9470 psi @Strain 0.730 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 72.39 MPa @Strain 0.770 %, Temperature -40.0 °C |
10500 psi @Strain 0.770 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 75.33 MPa @Strain 3.49 %, Temperature 90.0 °C |
10930 psi @Strain 3.49 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 79.52 MPa @Strain 1.49 %, Temperature 23.0 °C |
11530 psi @Strain 1.49 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 85.03 MPa @Strain 2.63 %, Temperature 40.0 °C |
12330 psi @Strain 2.63 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 87.13 MPa @Strain 1.11 %, Temperature 0.000 °C |
12640 psi @Strain 1.11 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 88.37 MPa @Strain 5.52 %, Temperature 90.0 °C |
12820 psi @Strain 5.52 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 98.25 MPa @Strain 0.940 %, Temperature -40.0 °C |
14250 psi @Strain 0.940 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 98.66 MPa @Strain 1.70 %, Temperature 40.0 °C |
14310 psi @Strain 1.70 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 102.87 MPa @Strain 1.34 %, Temperature 23.0 °C |
14920 psi @Strain 1.34 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 103.81 MPa @Strain 2.37 %, Temperature 23.0 °C |
15056 psi @Strain 2.37 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 109.37 MPa @Strain 1.34 %, Temperature 0.000 °C |
15863 psi @Strain 1.34 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 113.84 MPa @Strain 1.31 %, Temperature -40.0 °C |
16511 psi @Strain 1.31 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 121.6 MPa @Strain 1.79 %, Temperature 0.000 °C |
17640 psi @Strain 1.79 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 123.05 MPa @Strain 2.83 %, Temperature 40.0 °C |
17847 psi @Strain 2.83 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 135.14 MPa @Strain 2.05 %, Temperature 23.0 °C |
19600 psi @Strain 2.05 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 148.56 MPa @Strain 2.06 %, Temperature 0.000 °C |
21547 psi @Strain 2.06 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 150.01 MPa @Strain 1.54 %, Temperature -40.0 °C |
21757 psi @Strain 1.54 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 151.29 MPa @Strain 1.91 %, Temperature -40.0 °C |
21943 psi @Strain 1.91 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 191.87 MPa @Strain 2.24 %, Temperature -40.0 °C |
27828 psi @Strain 2.24 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| Elongation at Break | 5.0 % | 5.0 % | DAM; ISO 527-1/-2 |
| 7.0 % | 7.0 % | 50%RH; ISO 527-1/-2 | |
| Tensile Modulus | 6.50 GPa | 943 ksi | 50%RH; ISO 527-1/-2 |