Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

DuPont™ Nomex® Type 994, 125 mil Nominal Thickness Rigid Aromatic Nylon Board

Category Polymer , Thermoplastic , Nylon , Nylon, Aromatic
Manufacturer DuPont
Trade Name Nomex®
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF DuPont™ Nomex® Type 994, 125 mil Nominal Thickness Rigid Aromatic Nylon Board.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Type 994 is a densified, rigid board which has a unique combination of superior resistance to compression, even at elevated temperatures, along with relatively high oil absorption characteristics. This combination results in a product which is especially useful as spacers or other structural components in liquid-filled systems.Information provided by DuPont
Physical Properties Metric English Comments
Density 1.15 g/cc
0.0415 lb/in³
Calculated number using basis weight and thickness
Thickness 3180 microns
125 mil
ASTM D374, method D, using 17 N/cm²
Linear Mold Shrinkage 0.00 cm/cm
<br>@Temperature 240 °C
0.00 in/in
<br>@Temperature 464 °F
ASTM D3392
Linear Mold Shrinkage, Transverse 0.00 cm/cm
<br>@Temperature 240 °C
0.00 in/in
<br>@Temperature 464 °F
ASTM D3392
Mechanical Properties Metric English Comments
Hardness, Shore D 84
84
ASTM D2240
Film Tensile Strength at Yield, MD 107 MPa
15500 psi
ASTM D828
Film Tensile Strength at Yield, TD 93.0 MPa
13500 psi
ASTM D828
Flexural Strength 8.00 MPa
1160 psi
XD; ASTM D790
9.00 MPa
1310 psi
MD; ASTM D790
Flexural Modulus 0.255 GPa
37.0 ksi
XD; ASTM D790
0.360 GPa
52.2 ksi
MD; ASTM D790
Izod Impact, Unnotched 3.75 J/cm
7.03 ft-lb/in
XD; ASTM D256
5.45 J/cm
10.2 ft-lb/in
MD; ASTM D256
Compression Set 0.30 %
0.30 %
ASTM D3392
Thermal Properties Metric English Comments
Thermal Conductivity 0.160 W/m-K
<br>@Temperature 50.0 °C
1.11 BTU-in/hr-ft²-°F
<br>@Temperature 122 °F
ASTM D1674
0.161 W/m-K
<br>@Temperature 100 °C
1.12 BTU-in/hr-ft²-°F
<br>@Temperature 212 °F
ASTM D1674
0.163 W/m-K
<br>@Temperature 150 °C
1.13 BTU-in/hr-ft²-°F
<br>@Temperature 302 °F
ASTM D1674
0.165 W/m-K
<br>@Temperature 200 °C
1.15 BTU-in/hr-ft²-°F
<br>@Temperature 392 °F
ASTM D1674
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+16 ohm-cm
1.00e+16 ohm-cm
in air; ASTM D257
1.00e+15 ohm-cm
<br>@Temperature 125 °C
1.00e+15 ohm-cm
<br>@Temperature 257 °F
in oil; ASTM D257
1.00e+17 ohm-cm
<br>@Temperature 25.0 °C
1.00e+17 ohm-cm
<br>@Temperature 77.0 °F
in oil; ASTM D257
Surface Resistivity per Square 1.00e+17 ohm
1.00e+17 ohm
in air; ASTM D257
Dielectric Constant 3.5
<br>@Frequency 60.0 Hz
3.5
<br>@Frequency 60.0 Hz
in air; ASTM D150
4.0
<br>@Frequency 60.0 Hz,<br> Temperature 25.0 °C
4.0
<br>@Frequency 60.0 Hz,<br> Temperature 77.0 °F
in oil; ASTM D150
4.4
<br>@Frequency 60.0 Hz,<br> Temperature 125 °C
4.4
<br>@Frequency 60.0 Hz,<br> Temperature 257 °F
in oil; ASTM D150
Dielectric Strength 27.0 kV/mm
686 kV/in
AC rapid rise in oil; ASTM D149, 50mm electrodes
70.0 kV/mm
1780 kV/in
Full wave impulse in oil; ASTM D3426
Dissipation Factor 0.0070
<br>@Frequency 60.0 Hz
0.0070
<br>@Frequency 60.0 Hz
in air; ASTM D150
0.011
<br>@Frequency 60.0 Hz,<br> Temperature 25.0 °C
0.011
<br>@Frequency 60.0 Hz,<br> Temperature 77.0 °F
in oil; ASTM D150
0.016
<br>@Frequency 60.0 Hz,<br> Temperature 125 °C
0.016
<br>@Frequency 60.0 Hz,<br> Temperature 257 °F
in oil; ASTM D150
Descriptive Properties Value Comments
Basis Weight (g/m²) ASTM D3394
Compressibility (%) 1.1
ASTM D3392
Copyright © lookpolymers.com All Rights Reserved