Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Asahi Kasei Thermylene® P6-20FG-1734 20% Glass Fiber Reinforced, High Impact

Category Polymer , Thermoplastic , Polypropylene (PP) , Polypropylene with 20% Glass Fiber Filler
Manufacturer Asahi Kasei
Trade Name Thermylene®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Asahi Kasei Thermylene® P6-20FG-1734 20% Glass Fiber Reinforced, High Impact.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Information provided by Asahi Thermofil
Physical Properties Metric English Comments
Specific Gravity 1.04 g/cc
1.04 g/cc
ASTM D792
Linear Mold Shrinkage 0.0040 cm/cm
0.0040 in/in
ASTM D955
Melt Flow 2.5 g/10 min
2.5 g/10 min
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Rockwell R 84
84
ASTM D785
Tensile Strength, Yield 60.7 MPa
8800 psi
ASTM D638
Elongation at Yield 5.0 %
5.0 %
ASTM D638
Flexural Strength 79.3 MPa
11500 psi
ASTM D790
Flexural Modulus 2.96 GPa
430 ksi
ASTM D790
Izod Impact, Notched 1.60 J/cm
3.00 ft-lb/in
ASTM D256
Izod Impact, Unnotched 5.87 J/cm
11.0 ft-lb/in
ASTM D4812
Thermal Properties Metric English Comments
CTE, linear 43.2 µm/m-°C

@Temperature 20.0 °C
24.0 µin/in-°F

@Temperature 68.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 154 °C
310 °F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 143 °C
290 °F
ASTM D648