Styron EMERGEâ„¢ 4510-6 Polycarbonate

Category Polymer , Thermoplastic , Polycarbonate (PC)
Manufacturer Styron
Trade Name EMERGE™
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Styron EMERGEâ„¢ 4510-6 Polycarbonate.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
EMERGEâ„¢ PC 4510-6 advanced resin is a general purpose polycarbonate resin offering ignition resistance, heat resistance and excellent toughness. Applications: Consumer Electronics and Information Technology Equipment Computer and Business Equipment Portable Electronics Information provided by DowThis product line was spun off from Dow Chemical to Styron in 2010.
Physical Properties Metric English Comments
Specific Gravity 1.20 g/cc
1.20 g/cc
ASTM D792
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm
0.0050 - 0.0070 in/in
ASTM D955
Melt Flow 6.0 g/10 min

@Load 1.20 kg,
Temperature 300 °C
6.0 g/10 min

@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 72.4 MPa
10500 psi
0.125 in, injection molded, unannealed; ASTM D638
Tensile Strength, Yield 60.0 MPa
8700 psi
0.125 in, injection molded, unannealed; ASTM D638
Elongation at Break 150 %
150 %
0.125 in, injection molded, unannealed; ASTM D638
Tensile Modulus 2.30 GPa
334 ksi
0.125 in, injection molded, unannealed; ASTM D638
Flexural Strength 96.5 MPa
14000 psi
0.125 in, injection molded, unannealed; ASTM D790
Flexural Modulus 2.41 GPa
350 ksi
0.125 in, injection molded, unannealed; ASTM D790
Izod Impact, Notched 9.08 J/cm
17.0 ft-lb/in
ASTM D256
Izod Impact, Unnotched NB
NB
ASTM D256
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 142 °C
288 °F
0.157 in, annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 122 °C
252 °F
0.157 in, unannealed; ASTM D648
139 °C
282 °F
0.157 in, annealed; ASTM D648
Vicat Softening Point 148 °C
298 °F
50°C/hr, 50N; ASTM D1525
Flammability, UL94 V-2
V-2
0.0625 in
V-2
V-2
0.125 in
Processing Properties Metric English Comments
Melt Temperature 299 - 327 °C
570 - 621 °F
Mold Temperature 77.0 - 110 °C
171 - 230 °F
Drying Temperature 121 °C
250 °F
Dry Time 3 - 4 hour
3 - 4 hour