Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay Specialty Polymers AvaSpire® AV-651 GF30 Polyaryletherketone (PAEK), 30% Glass Fiber

Category Polymer , Thermoplastic , Polyketone , Polyaryletherketone (PAEK), Glass Fiber Filled
Manufacturer Solvay Specialty Polymers
Trade Name AvaSpire®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay Specialty Polymers AvaSpire® AV-651 GF30 Polyaryletherketone (PAEK), 30% Glass Fiber.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
AvaSpire® AV-651 GF30 is a 30% glass fiber reinforced polyaryletherketone (PAEK) that has been specifically formulated to provide higher mechanical strength and stiffness than unfilled AV-651 resin. This resin offers chemical resistance nearly equivalent to glass fiber-reinforced PEEK in most chemicals, with a lower heat deflection temperature.Features: Autoclave Sterilizable; Biocompatible; E-beam Sterilizable; Ethylene Oxide Sterilizable; Fatigue Resistant; Flame Retardant; Good Chemical Resistance; Good Dimensional Stability; Good Sterilizability; Heat Sterilizable; High Heat Resistance; High Stiffness; High Strength; Radiation (Gamma) Resistant; Radiation Sterilizable; Radiotranslucent; Steam Resistant; Steam SterilizableUses: Aircraft Applications; Connectors; Dental Applications; Electrical/Electronic Applications; Film; Hospital Goods; Industrial Applications; Medical Devices; Medical/Healthcare Applications; Seals; Surgical InstrumentsInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Density 1.52 g/cc
0.0549 lb/in³
ASTM D792
Filler Content 30 %
30 %
Glass Fiber
Water Absorption 0.20 %

@Time 86400 sec
0.20 %

@Time 24.0 hour
ISO 62
Viscosity 410000 cP

@Shear Rate 1000 1/s,
Temperature 400 °C
410000 cP

@Shear Rate 1000 1/s,
Temperature 752 °F
Melt Viscosity; ASTM D3835
Linear Mold Shrinkage, Flow 0.0020 - 0.0040 cm/cm

@Thickness 3.18 mm
0.0020 - 0.0040 in/in

@Thickness 0.125 in
Linear Mold Shrinkage, Transverse 0.013 - 0.015 cm/cm

@Thickness 3.18 mm
0.013 - 0.015 in/in

@Thickness 0.125 in
ASTM D955
Melt Flow 9.0 g/10 min

@Load 2.16 kg,
Temperature 400 °C
9.0 g/10 min

@Load 4.76 lb,
Temperature 752 °F
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Rockwell M 101
101
ASTM D785
Tensile Strength 156 MPa
22600 psi
5 mm/min; ASTM D638
Tensile Strength, Yield 162 MPa

@Thickness 5.00 mm
23500 psi

@Thickness 0.197 in
5 mm/min, Type 1A; ISO 527-2
Elongation at Break 2.9 %
2.9 %
Type 1A, 5 mm/min; ISO 527-2
2.9 %
2.9 %
5 mm/min; ASTM D638
Tensile Modulus 9.90 GPa
1440 ksi
5 mm/min; ASTM D638
10.4 GPa
1510 ksi
ISO 527-2
Flexural Strength 228 MPa
33100 psi
ISO 178
234 MPa
33900 psi
ASTM D790
Flexural Modulus 9.40 GPa
1360 ksi
ASTM D790
9.70 GPa
1410 ksi
ISO 178
Compressive Strength 168 MPa
24400 psi
ASTM D695
Shear Strength 82.6 MPa
12000 psi
ASTM D732
Izod Impact, Notched 1.10 J/cm
2.06 ft-lb/in
ASTM D256
Izod Impact, Unnotched 9.60 J/cm
18.0 ft-lb/in
ASTM D256
Izod Impact, Notched (ISO) 12.0 kJ/m²
5.71 ft-lb/in²
ISO 180
Izod Impact, Unnotched (ISO) 64.0 kJ/m²
30.5 ft-lb/in²
ISO 180
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 17.0 µm/m-°C

@Temperature -50.0 - 50.0 °C
9.44 µin/in-°F

@Temperature -58.0 - 122 °F
1
Specific Heat Capacity 1.27 J/g-°C

@Temperature 50.0 °C
0.304 BTU/lb-°F

@Temperature 122 °F
ASTM C351
1.65 J/g-°C

@Temperature 200 °C
0.394 BTU/lb-°F

@Temperature 392 °F
ASTM C351
Thermal Conductivity 0.300 W/m-K
2.08 BTU-in/hr-ft²-°F
ASTM C177
Melting Point 345 °C
653 °F
ASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 213 °C
415 °F
Annealed; ASTM D648
Glass Transition Temp, Tg 158 °C
316 °F
DSC
Flammability, UL94 V-1

@Thickness 0.800 mm
V-1

@Thickness 0.0315 in
V-0

@Thickness 1.60 mm
V-0

@Thickness 0.0630 in
Electrical Properties Metric English Comments
Volume Resistivity 2.00e+17 ohm-cm
2.00e+17 ohm-cm
ASTM D257
Surface Resistance >= 1.90e+17 ohm
>= 1.90e+17 ohm
ASTM D257
Dielectric Constant 3.58

@Frequency 1.00e+6 Hz
3.58

@Frequency 1.00e+6 Hz
ASTM D150
3.61

@Frequency 60.0 Hz
3.61

@Frequency 60.0 Hz
ASTM D150
3.63

@Frequency 1000 Hz
3.63

@Frequency 1000 Hz
ASTM D150
Dielectric Strength 17.0 kV/mm

@Thickness 3.00 mm
432 kV/in

@Thickness 0.118 in
ASTM D149
Dissipation Factor 0.00

@Frequency 1000 Hz
0.00

@Frequency 1000 Hz
ASTM D150
0.0020

@Frequency 60.0 Hz
0.0020

@Frequency 60.0 Hz
ASTM D150
0.0040

@Frequency 1.00e+6 Hz
0.0040

@Frequency 1.00e+6 Hz
ASTM D150
Processing Properties Metric English Comments
Rear Barrel Temperature 365 °C
689 °F
Middle Barrel Temperature 371 °C
700 °F
Front Barrel Temperature 377 °C
711 °F
Nozzle Temperature 382 °C
720 °F
Melt Temperature 366 - 388 °C
691 - 730 °F
Mold Temperature 160 - 190 °C
320 - 374 °F
Drying Temperature 149 °C

@Time 14400 sec
300 °F

@Time 4.00 hour
Descriptive Properties Value Comments
Agency Ratings ISO 10993; ISO 10993-Part 1
Availability Africa & Middle East
Asia Pacific
Europe
Latin America
North America
Color Beige; Black
Form Pellets
Injection Rate Fast
Processing Technique Injection Molding; Machining; Profile Extrusion