Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

S&E Specialty Polymers GA-1050-OR3-LF PVC

Category Polymer , Thermoplastic , Vinyl (PVC) , PVC, Uncompounded
Manufacturer S&E Specialty Polymers
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF S&E Specialty Polymers GA-1050-OR3-LF PVC.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Application: Lead free, 105° C PVC insulating compound designed for SJEOO applications. Complies with RoHS requirements.Information provided by S&E Specialty Polymers
Physical Properties Metric English Comments
Specific Gravity 1.27 - 1.33 g/cc
1.27 - 1.33 g/cc
ASTM D792
Mechanical Properties Metric English Comments
Hardness, Shore A 78 - 86
78 - 86
ASTM D2240
Tensile Strength 17.8 MPa
2580 psi
ASTM D412
15.66 MPa

@Treatment Temp. 136 °C,
Time 605000 sec
2271 psi

@Treatment Temp. 277 °F,
Time 168 hour
Oven aged
15.66 MPa

@Treatment Temp. 60.0 °C,
Time 605000 sec
2271 psi

@Treatment Temp. 140 °F,
Time 168 hour
Elongation at Break 280 %
280 %
ASTM D412
291.2 %

@Treatment Temp. 136 °C,
Time 605000 sec
291.2 %

@Treatment Temp. 277 °F,
Time 168 hour
Oven aged
305.2 %

@Treatment Temp. 60.0 °C,
Time 605000 sec
305.2 %

@Treatment Temp. 140 °F,
Time 168 hour
100% Modulus 0.00965 GPa
1.40 ksi
ASTM D412
Thermal Properties Metric English Comments
Brittleness Temperature -24.0 °C
-11.2 °F
ASTM D746
Oxygen Index 27 %
27 %
ASTM D2863
Electrical Properties Metric English Comments
Volume Resistivity 2.00e+14 ohm-cm
2.00e+14 ohm-cm
wet; ASTM D257
5.00e+14 ohm-cm
5.00e+14 ohm-cm
dry; ASTM D257