| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Dart Drop, Total Energy | 7.00 - 50.0 J | 5.16 - 36.9 ft-lb | Average value: 37.2 J Grade Count:14 |
|
Overview of materials for Polycarbonate/ASA Alloy, Unreinforced
This property data is a summary of similar materials in the MatWeb database for the category "Polycarbonate/ASA Alloy, Unreinforced". Each property range of values reported is minimum and maximum va..
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP KL004A Acetal Homopolymer
LNP LUBRICOMP* KL004A is a compound based on Acetal Homopolymer resin containing 20% PTFE. Added feature of this material is: Wear Resistant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP RFL33 PA 66
LNP* LUBRICOMP* RFL33 is a compound based on Nylon 66 resin containing 15% Glass Fiber, 15% PTFE. Added feature of this material is: Wear Resistant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP RFP36 PA 66
LNP* LUBRICOMP* RFP36 is a compound based on Nylon 66 resin containing 30% Glass Fiber, 15% PTFE, Silicone. Added features of this material include: Wear Resistant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP RFP36XXZ PA 66 (Asia Pacific)
LNP Lubricomp RFP36XXZ is a compound based on Nylon 66 resin containing Glass Fiber, PTFE, Silicone. Added features of this material include: internally lubricated. Also known as Lubricomp RFL-4536 ..
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP WFL33 PBT
LNP* LUBRICOMP* WFL33 is a compound based on PBT containing 15% Glass Fiber, 15% PTFE. Added feature of this grade is: Wear Resistant.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP WFL34 PBT
LNP LUBRICOMP* WFL34 is a compound based on PBT resin containing 20% Glass Fiber, 15% PTFE. Added feature of this grade is: Wear Resistant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP WFP36 PBT
LNP LUBRICOMP* WFP36 is a compound based on PBT resin containing 30% Glass Fiber, 15% PTFE/Silicone. Added features of this material include: Wear Resistant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP LUBRICOMP WFP36 PBT (Asia Pacific)
LNP LUBRICOMP* WFP36 is a compound based on Polybutylene Terephalate resin containing Silicone, Glass Fiber, PTFE. Added features of this material include: Internally Lubricated.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP STAT-KON DDF029 PC (Asia Pacific)
LNP STAT-KON* DDF029 is a compound based on Polycarbonate resin containing Carbon Powder, Flame Retardant, Glass Fiber. Added features of this material include: Electrically Conductive.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics Valox® 830F PBT+PET
PBT+PET, 30% Glass, Mold Release, Heat Stabilized, For food contact applications
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics Valox® IQ420 PBT (Asia Pacific)
Environmentally responsible Valox iQ420 resin: iQ-PBT+ 30% glass fiber reinforcement. Targeted for use in electrical motors, connectors, pump housings, spotlights, appliance handles, etc.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics Valox® IQ420 PBT (Europe-Africa-Middle East)
Environmentally responsible Valox iQ420 resin: iQ-PBT+ 30% glass fiber reinforcement. Targeted for use in electrical motors, connectors, pump housings, spotlights, appliance handles, etc.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics Valox® IQ507 PBT+PC
Valox iQ507 resin: Environmentally responsible, sustainable, and low carbon footprint resin that is 30% glass fiber reinforced PBT+PC alloy. Valox iQ507 offers good mechanical and thermal characte..
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | ASTM D3763 |
|
SABIC Innovative Plastics Valox® K4560 PBT
30% glass reinforced PBT. Impact modified, high flow, hydrolytically stable.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP EC006 PEI
LNP THERMOCOMP* EC006 is a compound based on Polyetherimide resin containing 30% Carbon Fiber. Added features of this material include: Electrically Conductive.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP EC008PXQ PEI
LNP* THERMOCOMP* EC008PXQ is a compound based on Polyetherimide containing 40% Carbon FIber. Added features include: Electrically Conductive, Exceptional Processing
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP KZ001L Acetal Copoly
LNP* THERMOCOMP* KZ001L is a compound based on Acetal Copolymer resin containing 5% Milled Glass. Added features of this material include: Low Extractible.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP LC00APXQ PEEK
LNP* THERMOCOMP* LC00APXQ is a compound based on Polyetheretherketone resin containing 50% Carbon Fiber. Added features of this material include: Exceptional Processing, Electrically Conductive.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP RF004XXH PA 66
LNP THERMOCOMP* RF004XXH is a compound based on Nylon 66 resin containing 20% Glass Fiber. Added feature of this grade is: Healthcare.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP RFB53XXZ PA 66
LNP* THERMOCOMP* RFB53XXZ is a compound based on Nylon 66 resin containing 15% Glass Fiber, 25% Glass Bead.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP RX96592 PA 66
LNP* Thermocomp* RX96592 is a compound based on Nylon 6/6 containing Proprietary Fillers.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP UC008H PPA (Asia Pacific)
LNP* THERMOCOMP* UC008H is a compound based on Polyphthalamide resin containing Carbon Fiber. Added features of this material include: Electrically Conductive.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP UF006H PPA
LNP* THERMOCOMP* UF006H is a compound based on Polyphthalamide resin containing 30% Glass Fiber. Added feature of this grade is: Healthcare.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP STAT-KON DDF029 PC
LNP STAT-KON* DDF029 is a compound based on Polycarbonate resin containing Carbon, Glass Fiber. Added features of this material include: Electrically Conductive. Flame Retardant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP RFZ349XC PA 66 (Asia Pacific)
LNP* THERMOCOMP* RFZ349XC is a compound based on Nylon 66 resin containing Glass Fiber, Milled Glass. Added features of this material include: Flame Retardant.
|
|||
| Dart Drop, Total Energy | 7.00 J | 5.16 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
|
SABIC Innovative Plastics LNP VERTON MX02795 PP
LNP* VERTON* MX02795 is a compound based on Polypropylene resin containing Proprietary Fillers. Added features of this material include: Heat Stabilized, UV Stabilized, Structural.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics NORYL GTX GTX675 PPE+PA6
Noryl GTX* GTX675 Resin is a blend of Polyphenylene Ether(PPE) + Polyamide(PA) resin that is mineral filled, conductive, and suitable for injection molding. The conductivity level is optimized to a..
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP STAT-KON OE002 PPS - LINEAR
LNP* STAT-KON* OE002 is a compound based on PPS - Linear resin containing 10% Carbon Fiber. Added feature of this material is: Electrically Conductive.
|
|||
| Dart Drop, Total Energy |
7.00
J <br>@Temperature 23.0 °C
|
5.16
ft-lb <br>@Temperature 73.4 °F
|
ASTM D3763 |
|
SABIC Innovative Plastics LNP THERMOCOMP RF007SXN PA 66
LNP* THERMOCOMP* RF007SXN is a Hydro-Stable, 35% Glass Fiber reinforced compound based on Nylon 66. Added features of this grade include: Heat Stabilized, NSF Listed.
|
|||