Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Overview of materials for Polyetherimide (PEI), Aramid Fiber Filled

Category Polymer , Thermoplastic , Polyetherimide (PEI) , Polyetherimide (PEI), Aramid Fiber Filled
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polyetherimide (PEI), Aramid Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyetherimide, Aramid Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.28 - 1.38 g/cc
0.0462 - 0.0499 lb/in³
Average value: 1.32 g/cc Grade Count:7
Water Absorption 0.100 - 0.200 %
0.100 - 0.200 %
Average value: 0.183 % Grade Count:6
Linear Mold Shrinkage 0.00300 - 0.00700 cm/cm
0.00300 - 0.00700 in/in
Average value: 0.00479 cm/cm Grade Count:7
Mechanical Properties Metric English Comments
Hardness, Rockwell R 125
125
Average value: 125 Grade Count:3
Tensile Strength, Ultimate 82.7 - 100 MPa
12000 - 14500 psi
Average value: 91.9 MPa Grade Count:7
Elongation at Break 2.50 - 8.10 %
2.50 - 8.10 %
Average value: 4.80 % Grade Count:7
Modulus of Elasticity 3.03 - 4.83 GPa
439 - 700 ksi
Average value: 4.13 GPa Grade Count:7
Flexural Yield Strength 124 - 145 MPa
18000 - 21000 psi
Average value: 136 MPa Grade Count:7
Flexural Modulus 3.45 - 4.14 GPa
500 - 600 ksi
Average value: 3.89 GPa Grade Count:7
Izod Impact, Notched 0.267 - 0.534 J/cm
0.500 - 1.00 ft-lb/in
Average value: 0.450 J/cm Grade Count:7
Izod Impact, Unnotched 2.67 - 5.34 J/cm
5.00 - 10.0 ft-lb/in
Average value: 4.10 J/cm Grade Count:7
Thermal Properties Metric English Comments
CTE, linear 25.2 - 30.6 µm/m-°C
14.0 - 17.0 µin/in-°F
Average value: 28.2 µm/m-°C Grade Count:3
Thermal Conductivity 0.231 - 0.245 W/m-K
1.60 - 1.70 BTU-in/hr-ft²-°F
Average value: 0.238 W/m-K Grade Count:4
Deflection Temperature at 0.46 MPa (66 psi) 210 - 213 °C
410 - 415 °F
Average value: 212 °C Grade Count:5
Deflection Temperature at 1.8 MPa (264 psi) 185 - 204 °C
365 - 400 °F
Average value: 201 °C Grade Count:7
Flammability, UL94 V-0
V-0
Grade Count:6
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+14 - 1.00e+16 ohm-cm
1.00e+14 - 1.00e+16 ohm-cm
Average value: 8.35e+15 ohm-cm Grade Count:6
Processing Properties Metric English Comments
Processing Temperature 349 - 382 °C
660 - 720 °F
Average value: 366 °C Grade Count:5
Mold Temperature 121 - 177 °C
250 - 350 °F
Average value: 153 °C Grade Count:7
Injection Pressure 82.7 - 124 MPa
12000 - 18000 psi
Average value: 103 MPa Grade Count:6
Users viewing this material also viewed the following: