| Category | Metal , Ferrous Metal , Austenitic , Stainless Steel |
| Manufacturer | Outokumpu |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | Outokumpu 4436 Cr-Ni-Mo Austenitic Stainless Steel.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 8.00 g/cc | 0.289 lb/in³ | RT |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Brinell | 165 | 165 | Outokumpu Typical, 20°C, Hot rolled plate (Quarto)/Cold rolled strip/sheet; EN 10003-1 |
| Tensile Strength, Ultimate | 590 MPa | 85600 psi | Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1 |
| 360 MPa @Temperature 500 °C |
52200 psi @Temperature 932 °F |
EN min.; EN 10002-5 | |
| 380 MPa @Temperature 300 °C |
55100 psi @Temperature 572 °F |
EN min.; EN 10002-5 | |
| 380 MPa @Temperature 400 °C |
55100 psi @Temperature 752 °F |
EN min.; EN 10002-5 | |
| 390 MPa @Temperature 200 °C |
56600 psi @Temperature 392 °F |
EN min.; EN 10002-5 | |
| 430 MPa @Temperature 100 °C |
62400 psi @Temperature 212 °F |
EN min.; EN 10002-5 | |
| 840 MPa @Temperature -80.0 °C |
122000 psi @Temperature -112 °F |
EN min; EN 10002-5 | |
| 1200 MPa @Temperature -196 °C |
174000 psi @Temperature -321 °F |
EN min; EN 10002-5 | |
| Tensile Strength, Yield | 220 MPa @Strain 0.200 % |
31900 psi @Strain 0.200 % |
EN min.,RT; EN 10002-1 |
| 300 MPa @Strain 0.200 % |
43500 psi @Strain 0.200 % |
Outokumpu Typical,Hot Rolled Plate (Quarto); EN 10002-1 | |
| 340 MPa @Strain 1.00 % |
49300 psi @Strain 1.00 % |
Outokumpu Typical,Hot Rolled Plate (Quarto); EN 10002-1 | |
| 100 MPa @Strain 0.200 %, Temperature 500 °C |
14500 psi @Strain 0.200 %, Temperature 932 °F |
EN min.; EN 10002-5 | |
| 108 MPa @Strain 0.200 %, Temperature 400 °C |
15700 psi @Strain 0.200 %, Temperature 752 °F |
EN min.; EN 10002-5 | |
| 118 MPa @Strain 0.200 %, Temperature 300 °C |
17100 psi @Strain 0.200 %, Temperature 572 °F |
EN min.; EN 10002-5 | |
| 128 MPa @Strain 1.00 %, Temperature 500 °C |
18600 psi @Strain 1.00 %, Temperature 932 °F |
EN min.; EN 10002-5 | |
| 135 MPa @Strain 1.00 %, Temperature 400 °C |
19600 psi @Strain 1.00 %, Temperature 752 °F |
EN min.; EN 10002-5 | |
| 137 MPa @Strain 0.200 %, Temperature 200 °C |
19900 psi @Strain 0.200 %, Temperature 392 °F |
EN min.; EN 10002-5 | |
| 145 MPa @Strain 1.00 %, Temperature 300 °C |
21000 psi @Strain 1.00 %, Temperature 572 °F |
EN min.; EN 10002-5 | |
| 166 MPa @Strain 0.200 %, Temperature 100 °C |
24100 psi @Strain 0.200 %, Temperature 212 °F |
EN min.; EN 10002-5 | |
| 167 MPa @Strain 1.00 %, Temperature 200 °C |
24200 psi @Strain 1.00 %, Temperature 392 °F |
EN min.; EN 10002-5 | |
| 199 MPa @Strain 1.00 %, Temperature 100 °C |
28900 psi @Strain 1.00 %, Temperature 212 °F |
EN min.; EN 10002-5 | |
| 275 MPa @Strain 0.200 %, Temperature -80.0 °C |
39900 psi @Strain 0.200 %, Temperature -112 °F |
EN min.; EN 10002-5 | |
| 350 MPa @Strain 0.200 %, Temperature -196 °C |
50800 psi @Strain 0.200 %, Temperature -321 °F |
EN min.; EN 10002-5 | |
| 355 MPa @Strain 1.00 %, Temperature -80.0 °C |
51500 psi @Strain 1.00 %, Temperature -112 °F |
EN min.; EN 10002-5 | |
| 450 MPa @Strain 1.00 %, Temperature -196 °C |
65300 psi @Strain 1.00 %, Temperature -321 °F |
EN min.; EN 10002-5 | |
| Elongation at Break | 50 % | 50 % | Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1 |
| 35 % @Temperature -196 °C |
35 % @Temperature -321 °F |
EN min | |
| 40 % @Temperature -80.0 °C |
40 % @Temperature -112 °F |
EN min | |
| Modulus of Elasticity | 200 GPa | 29000 ksi | RT |
| 165 GPa @Temperature 500 °C |
23900 ksi @Temperature 932 °F |
||
| 172 GPa @Temperature 400 °C |
24900 ksi @Temperature 752 °F |
||
| 179 GPa @Temperature 300 °C |
26000 ksi @Temperature 572 °F |
||
| 186 GPa @Temperature 200 °C |
27000 ksi @Temperature 392 °F |
||
| 194 GPa @Temperature 100 °C |
28100 ksi @Temperature 212 °F |
||
| Poissons Ratio | 0.30 | 0.30 | RT |
| Shear Modulus | 77.0 GPa | 11200 ksi | calculated |
| Impact Test | >= 60.0 J | >= 44.3 ft-lb | Hot rolled plate/Cold rolled strip/sheet, 10x10mm test pieces; EN 10045-1 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 16.0 µm/m-°C @Temperature 100 °C |
8.89 µin/in-°F @Temperature 212 °F |
|
| 16.5 µm/m-°C @Temperature 200 °C |
9.17 µin/in-°F @Temperature 392 °F |
||
| 17.0 µm/m-°C @Temperature 300 °C |
9.44 µin/in-°F @Temperature 572 °F |
||
| 17.5 µm/m-°C @Temperature 400 °C |
9.72 µin/in-°F @Temperature 752 °F |
||
| 18.0 µm/m-°C @Temperature 500 °C |
10.0 µin/in-°F @Temperature 932 °F |
||
| Specific Heat Capacity | 0.500 J/g-°C | 0.120 BTU/lb-°F | RT |
| Thermal Conductivity | 15.0 W/m-K | 104 BTU-in/hr-ft²-°F | RT |
| 20.0 W/m-K @Temperature 400 °C |
139 BTU-in/hr-ft²-°F @Temperature 752 °F |
| Component Elements Properties | Metric | English | Comments |
|---|---|---|---|
| Carbon, C | 0.040 % | 0.040 % | |
| Chromium, Cr | 16.9 % | 16.9 % | |
| Iron, Fe | 69.76 % | 69.76 % | |
| Molybdenum, Mo | 2.6 % | 2.6 % | |
| Nickel, Ni | 10.7 % | 10.7 % |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.0000750 ohm-cm | 0.0000750 ohm-cm | RT |