Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Lubrizol ESTANE® 58134 Ester Based Thermoplastic Polyurethane (European Grade)

Category Polymer , Thermoplastic , Elastomer, TPE , Polyurethane, TP , Thermoplastic Polyurethane, Elastomer, Polyester Grade
Manufacturer Lubrizol (former Noveon)
Trade Name ESTANE®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Lubrizol ESTANE® 58134 Ester Based Thermoplastic Polyurethane (European Grade).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Description: Estane® thermoplastic polyurethanes (TPUs) include elastomeric materials that bridge the gap between flexible rubber and rigid plastics. These materials offer toughness and durability in a flexible thermoplastic elastomer system that is easy to process in a wide range of equipment. The Estane® TPU portfolio of products offers high performance polyester - and polyether - based resins and compounds in a broad range of hardnesses to meet a variety of application needs.Benefits of Estane® TPU: Outstanding Abrasion and Wear ResistanceExcellent Low Temperature FlexibilitySuperior Toughness and DurabilityEase of Processing and Manufacturing FlexibilityColorability and Paintability with no adhesion promoterApplications: Film & SheetFabric coating & melt coatingWire & CableHose, Tube & ProfileCustom moldingCustom compoundingAutomotive interior/chassis and exterior painted trimInformation provided by Noveon, Inc.
Physical Properties Metric English Comments
Specific Gravity 1.20 g/cc
1.20 g/cc
ISO 2781
Mechanical Properties Metric English Comments
Hardness, Shore A 88
88
ISO 868
Hardness, Shore D 40
40
ISO 868
Tensile Strength, Ultimate 51.0 MPa
7400 psi
ISO 37
Elongation at Break 530 %
530 %
ISO 37
Tensile Modulus 0.0350 GPa
5.08 ksi
ISO 527
50% Modulus 0.00610 GPa
0.885 ksi
ISO 37
100% Modulus 0.00700 GPa
1.02 ksi
ISO 37
300% Modulus 0.0143 GPa
2.07 ksi
ISO 37
Rebound 40 %
40 %
ISO 4662
Tear Strength 85.0 kN/m
485 pli
with incision; ISO 34B
102 kN/m
582 pli
without incision; ISO 34B
Abrasion 35
35
mm<sup>3</sup>; ISO 4649
Compression Set 22 %
22 %
70 hrs./22°C; ISO 815
51 %
51 %
24 hrs./70°C; ISO 815
Thermal Properties Metric English Comments
Vicat Softening Point 94.0 °C
201 °F
A50; ISO 306