Material Notes:
Features: Fast cycling, broad temperature performance, and durabilityUses: Injection MoldingAvailable in Americas, Europe, Middle East, Africa, India and AsiaInformation provided by Lubrizol
Physical Properties Metric English Comments
Specific Gravity 1.21 g/cc
1.21 g/cc
ASTM D792
Maximum Moisture Content 0.020
0.020
Linear Mold Shrinkage 0.0060 cm/cm
0.0060 in/in
flex bar
0.0090 cm/cm
0.0090 in/in
disk
Mechanical Properties Metric English Comments
Hardness, Shore A 87 - 93

@Time 5.00 sec
87 - 93

@Time 0.00139 hour
ASTM D2240
Tensile Strength 33.0 MPa
4790 psi
ASTM D412
Elongation at Break 645 %
645 %
ASTM D412
100% Modulus 0.00700 GPa
1.02 ksi
ASTM D412
300% Modulus 0.0170 GPa
2.47 ksi
ASTM D412
Flexural Modulus 0.0386 GPa
5.60 ksi
ASTM D790
Tear Strength 29.8 kN/m
170 pli
Trouser; ASTM D470
Graves Tear Strength 116 kN/m
660 pli
Die C; ASTM D624
Taber Abrasion, mg/1000 Cycles 45
45
CS-17, 1000g; ASTM D3389 B
Thermal Properties Metric English Comments
Melting Point 179 °C
354 °F
DSC
Glass Transition Temp, Tg -47.0 °C
-52.6 °F
DSC
Processing Properties Metric English Comments
Rear Barrel Temperature 200 °C
392 °F
Injection
Middle Barrel Temperature 204 °C
399 °F
Injection
Front Barrel Temperature 210 °C
410 °F
Injection
Nozzle Temperature 215 °C
419 °F
Injection
Melt Temperature 215 °C
419 °F
Injection
Drying Temperature 104 °C
219 °F
Dry Time 2.00 - 4.00 hour
2.00 - 4.00 hour
Dew Point -40.0 °C
-40.0 °F
Injection Pressure 68.9 - 103 MPa
10000 - 15000 psi
Injection
Hold Pressure 34.5 - 68.9 MPa
5000 - 10000 psi
Injection
Back Pressure >= 0.345 MPa
>= 50.0 psi
Injection
Screw Speed 60 - 100 rpm
60 - 100 rpm
Injection