Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Industrial Laminates/Norplex ES-1 Engraving Stock

Category Polymer , Thermoset
Manufacturer Industrial Laminates/Norplex
Trade Name
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Industrial Laminates/Norplex ES-1 Engraving Stock.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Description: Composed of white melamine paper core with various pigmented cover sheets.Thickness Tested: 0.0620”, 0.125”, and 0.500”
Physical Properties Metric English Comments
Specific Gravity >= 1.40 g/cc
>= 1.40 g/cc
Moisture Absorption at Equilibrium 2.5 %
<br>@Thickness 1.57 mm
2.5 %
<br>@Thickness 0.0620 in
Mechanical Properties Metric English Comments
Hardness, Rockwell M 90 - 110
<br>@Thickness 1.57 mm
90 - 110
<br>@Thickness 0.0620 in
Tensile Strength, Yield 63.4 MPa
<br>@Thickness 3.17 mm
9200 psi
<br>@Thickness 0.125 in
CW
72.4 MPa
<br>@Thickness 3.17 mm
10500 psi
<br>@Thickness 0.125 in
LW
Flexural Strength 93.1 MPa
<br>@Thickness 1.57 mm
13500 psi
<br>@Thickness 0.0620 in
CW
93.1 MPa
<br>@Thickness 1.57 mm
13500 psi
<br>@Thickness 0.0620 in
LW
Flexural Modulus 10.3 GPa
<br>@Thickness 1.57 mm
1500 ksi
<br>@Thickness 0.0620 in
CW
10.3 GPa
<br>@Thickness 1.57 mm
1500 ksi
<br>@Thickness 0.0620 in
LW
Compressive Strength 172 MPa
<br>@Thickness 12.7 mm
25000 psi
<br>@Thickness 0.500 in
Flatwise
Izod Impact, Unnotched 0.294 J/cm
<br>@Thickness 12.7 mm
0.550 ft-lb/in
<br>@Thickness 0.500 in
CW, E-48/50
0.320 J/cm
<br>@Thickness 12.7 mm
0.600 ft-lb/in
<br>@Thickness 0.500 in
LW, E-48/50
Thermal Properties Metric English Comments
CTE, linear 10.0 µm/m-°C
<br>@Temperature 20.0 °C
5.56 µin/in-°F
<br>@Temperature 68.0 °F
x-axis
CTE, linear, Transverse to Flow 14.0 µm/m-°C
<br>@Temperature 20.0 °C
7.78 µin/in-°F
<br>@Temperature 68.0 °F
y-axis
Maximum Service Temperature, Air 120 °C
248 °F
Maximum Operating Temperature
Flammability, UL94 V-1
V-1
Electrical Properties Metric English Comments
Dielectric Breakdown 5000 V
<br>@Thickness 1.57 mm
5000 V
<br>@Thickness 0.0620 in
D-48/50
50000 V
<br>@Thickness 1.57 mm
50000 V
<br>@Thickness 0.0620 in
Condition A
Arc Resistance 120 sec
<br>@Thickness 3.17 mm
120 sec
<br>@Thickness 0.125 in
ASTM D495
Descriptive Properties Value Comments
Bond Strength 1,000 lb
0.5&quot;