Information provided by HexCel
Mechanical Properties Metric English Comments
Tensile Strength, Yield 2170 MPa

@Temperature 25.0 °C
315000 psi

@Temperature 77.0 °F
0°, Dry
Elongation at Yield 1.4 %
1.4 %
0°, Dry
Tensile Modulus 145 GPa
21000 ksi
0°, Dry
Flexural Yield Strength 1700 MPa

@Temperature 25.0 °C
247000 psi

@Temperature 77.0 °F
0°, Dry
Flexural Modulus 123 GPa

@Temperature 25.0 °C
17800 ksi

@Temperature 77.0 °F
0°, Dry
Compressive Yield Strength 262 MPa

@Temperature 82.0 °C
38000 psi

@Temperature 180 °F
Open hole compression, Wet
303 MPa

@Temperature 25.0 °C
43900 psi

@Temperature 77.0 °F
After 1500 in-inlb/in impact, Dry
303 MPa

@Temperature 25.0 °C
43900 psi

@Temperature 77.0 °F
Open hole compression, Dry
1170 MPa

@Temperature 82.0 °C
170000 psi

@Temperature 180 °F
0°, Wet
1240 MPa

@Temperature 121 °C
180000 psi

@Temperature 250 °F
0°, Dry
1410 MPa

@Temperature 82.0 °C
205000 psi

@Temperature 180 °F
0°, Dry
1590 MPa

@Temperature 25.0 °C
231000 psi

@Temperature 77.0 °F
0°, Dry
Compressive Modulus 123 GPa

@Temperature 82.0 °C
17800 ksi

@Temperature 180 °F
0°, Wet
127 GPa

@Temperature 121 °C
18400 ksi

@Temperature 250 °F
0°, Dry
129 GPa

@Temperature 104 °C
18700 ksi

@Temperature 219 °F
0°, Wet
138 GPa

@Temperature 25.0 °C
20000 ksi

@Temperature 77.0 °F
0°, Dry
Shear Strength 50.3 MPa

@Temperature 121 °C
7300 psi

@Temperature 250 °F
Short Beam, Wet
65.5 MPa

@Temperature 121 °C
9500 psi

@Temperature 250 °F
Short Beam, Dry
82.7 MPa

@Temperature 82.0 °C
12000 psi

@Temperature 180 °F
Short Beam, Wet
84.8 MPa

@Temperature 82.0 °C
12300 psi

@Temperature 180 °F
Short Beam, Dry
107 MPa

@Temperature 25.0 °C
15500 psi

@Temperature 77.0 °F
Short Beam, Dry
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 93.3 °C
200 °F
Epoxy Matrix Limit