Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Haynes Hastelloy® C-2000® Nickel Alloy Shielded Metal Arc Welded (SMAW) All Weld Cruciform

Category Metal , Nonferrous Metal , Nickel Alloy
Manufacturer Haynes International, Inc.
Trade Name Hastelloy®
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Haynes Hastelloy® C-2000® Nickel Alloy Shielded Metal Arc Welded (SMAW) All Weld Cruciform.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Nickel-chromium-molybdenum (Ni-Cr-Mo) C-type alloys have a long history of use in the Chemical Process Industries and are known for their versatility. Not only do they resist all acids (especially hydrochloric, sulfuric, and hydrofluoric) over large temperature ranges, but they also resist the insidious types of attack induced by chlorides and other halide solutions, specifically pitting, crevice attack, and stress corrosion cracking. HASTELLOY® C-2000® alloy has greater versatility than traditional Ni-Cr-Mo alloys. This was accomplished by use of a high chromium content, a high molybdenum content, and a small but effective addition of copper. The copper provides enhanced temperature capability in sulfuric acid, hydrofluoric acid, and dilute hydrochloric acid.C-2000 alloy is available in plate, sheet, strip, billet, bar, wire, covered electrodes, pipe, and tubing. Applications: Chemical process industry reactors, heat exchangers, columns, and piping.Pharmaceutical industry reactors and dryers.Flue gas desulfurization systems.C-2000 alloy is covered by ASME, ASTM, AWS, DIN, and TÜV specifications.Welding: The weldability of C-2000 alloy is similar to that of C-276 alloy. To weld the C-type alloys, three processes are commonly used. For sheet welds and plate root passes, gas tungsten arc (GTAW) welding is favored. For plate welds, the gas metal arc (GMAW) process is preferred. For field welding, the shielded metal arc process, using coated electrodes, is favored. Submerged arc welding is not recommended as this process is characterized by high heat input to the base metal and slow cooling of the weld. To minimize the precipitation of second phases in regions affected by the heat of welding, a maximum interpass temperature of 93°C (200°F) is recommended for the C-type alloys. Welding of cold-worked materials is strongly discouraged, since they sensitize more quickly and induce residual stresses. A full solution anneal, followed by water quenching, is recommended for cold-worked structures prior to welding.Base Metal Preparation: The joint surface and adjacent area should be thoroughly cleaned before welding. All grease, oil, crayon marks, sulfur compounds, and other foreign matter should be removed. Filler Metal Selections: For gas tungsten arc and gas metal arc welding, C-2000 filler wire (ERNiCrMo-17) is suggested. For shielded metal arc welding,C-2000 covered electrodes (ENiCrMo-17) are suggested. Heat Treatment: The standard solution annealing treatment consists of heating to 1135°C (2075°F) followed by rapid air-cooling or water quenching. Parts which have been hot formed should be solution annealed prior to final fabrication or installation.Forming: C-2000 alloy has excellent forming characteristics, and cold forming is the preferred method of shaping. The alloy can be easily cold worked due to its good ductility. The alloy is generally stiffer than the austenitic stainless steels so more energy is required during cold forming.Tensile and impact properties reported are for welded samples. Other properties are typical of the alloy.Data provided by the manufacturer, Haynes International, Inc.
Physical Properties Metric English Comments
Density 8.50 g/cc
0.307 lb/in³
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 565 MPa
<br>@Diameter 12.7 mm,<br> Temperature 450 °C
81900 psi
<br>@Diameter 0.500 in,<br> Temperature 842 °F
744 MPa
<br>@Diameter 12.7 mm,<br> Temperature 25.0 °C
108000 psi
<br>@Diameter 0.500 in,<br> Temperature 77.0 °F
Tensile Strength, Yield 386 MPa
<br>@Diameter 12.7 mm,<br> Temperature 450 °C
56000 psi
<br>@Diameter 0.500 in,<br> Temperature 842 °F
0.2% offset
510 MPa
<br>@Diameter 12.7 mm,<br> Temperature 25.0 °C
74000 psi
<br>@Diameter 0.500 in,<br> Temperature 77.0 °F
0.2% offset
Elongation at Break 40.4 %
<br>@Diameter <=12.7 mm,<br> Temperature 25.0 °C
40.4 %
<br>@Diameter <=0.500 in,<br> Temperature 77.0 °F
43.9 %
<br>@Diameter <=12.7 mm,<br> Temperature 450 °C
43.9 %
<br>@Diameter <=0.500 in,<br> Temperature 842 °F
Modulus of Elasticity 162 GPa
<br>@Temperature 649 °C
23500 ksi
<br>@Temperature 1200 °F
171 GPa
<br>@Temperature 538 °C
24800 ksi
<br>@Temperature 1000 °F
177 GPa
<br>@Temperature 427 °C
25700 ksi
<br>@Temperature 801 °F
190 GPa
<br>@Temperature 316 °C
27600 ksi
<br>@Temperature 601 °F
207 GPa
<br>@Temperature 25.0 °C
30000 ksi
<br>@Temperature 77.0 °F
Charpy Impact 45.0 J
<br>@Temperature -196 °C
33.2 ft-lb
<br>@Temperature -321 °F
Metal Sample from Plate Weld
71.0 J
<br>@Temperature 25.0 °C
52.4 ft-lb
<br>@Temperature 77.0 °F
Metal Sample from Plate Weld
Thermal Properties Metric English Comments
CTE, linear 12.4 µm/m-°C
<br>@Temperature 25.0 - 200 °C
6.89 µin/in-°F
<br>@Temperature 77.0 - 392 °F
12.4 µm/m-°C
<br>@Temperature 25.0 - 100 °C
6.89 µin/in-°F
<br>@Temperature 77.0 - 212 °F
12.6 µm/m-°C
<br>@Temperature 25.0 - 300 °C
7.00 µin/in-°F
<br>@Temperature 77.0 - 572 °F
12.9 µm/m-°C
<br>@Temperature 25.0 - 400 °C
7.17 µin/in-°F
<br>@Temperature 77.0 - 752 °F
13.2 µm/m-°C
<br>@Temperature 25.0 - 500 °C
7.33 µin/in-°F
<br>@Temperature 77.0 - 932 °F
13.3 µm/m-°C
<br>@Temperature 25.0 - 600 °C
7.39 µin/in-°F
<br>@Temperature 77.0 - 1110 °F
Specific Heat Capacity 0.428 J/g-°C
<br>@Temperature 25.0 °C
0.102 BTU/lb-°F
<br>@Temperature 77.0 °F
0.434 J/g-°C
<br>@Temperature 100 °C
0.104 BTU/lb-°F
<br>@Temperature 212 °F
0.443 J/g-°C
<br>@Temperature 200 °C
0.106 BTU/lb-°F
<br>@Temperature 392 °F
0.455 J/g-°C
<br>@Temperature 300 °C
0.109 BTU/lb-°F
<br>@Temperature 572 °F
0.468 J/g-°C
<br>@Temperature 400 °C
0.112 BTU/lb-°F
<br>@Temperature 752 °F
0.486 J/g-°C
<br>@Temperature 500 °C
0.116 BTU/lb-°F
<br>@Temperature 932 °F
0.536 J/g-°C
<br>@Temperature 600 °C
0.128 BTU/lb-°F
<br>@Temperature 1110 °F
Thermal Conductivity 9.10 W/m-K
<br>@Temperature 25.0 °C
63.2 BTU-in/hr-ft²-°F
<br>@Temperature 77.0 °F
10.8 W/m-K
<br>@Temperature 100 °C
75.0 BTU-in/hr-ft²-°F
<br>@Temperature 212 °F
12.6 W/m-K
<br>@Temperature 200 °C
87.4 BTU-in/hr-ft²-°F
<br>@Temperature 392 °F
14.1 W/m-K
<br>@Temperature 300 °C
97.9 BTU-in/hr-ft²-°F
<br>@Temperature 572 °F
16.1 W/m-K
<br>@Temperature 400 °C
112 BTU-in/hr-ft²-°F
<br>@Temperature 752 °F
18.0 W/m-K
<br>@Temperature 500 °C
125 BTU-in/hr-ft²-°F
<br>@Temperature 932 °F
21.6 W/m-K
<br>@Temperature 600 °C
150 BTU-in/hr-ft²-°F
<br>@Temperature 1110 °F
Melting Point 1328 - 1358 °C
2422 - 2476 °F
Solidus 1328 °C
2422 °F
Liquidus 1358 °C
2476 °F
Component Elements Properties Metric English Comments
Aluminum, Al <= 0.50 %
<= 0.50 %
Carbon, C <= 0.010 %
<= 0.010 %
Chromium, Cr 23 %
23 %
Copper, Cu 1.6 %
1.6 %
Iron, Fe <= 3.0 %
<= 3.0 %
Manganese, Mn <= 0.50 %
<= 0.50 %
Molybdenum, Mo 16 %
16 %
Nickel, Ni >= 57 %
>= 57 %
as balance
Silicon, Si <= 0.080 %
<= 0.080 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.000128 ohm-cm
<br>@Temperature 25.0 °C
0.000128 ohm-cm
<br>@Temperature 77.0 °F
0.000129 ohm-cm
<br>@Temperature 100 °C
0.000129 ohm-cm
<br>@Temperature 212 °F
0.000130 ohm-cm
<br>@Temperature 200 °C
0.000130 ohm-cm
<br>@Temperature 392 °F
0.000131 ohm-cm
<br>@Temperature 300 °C
0.000131 ohm-cm
<br>@Temperature 572 °F
0.000132 ohm-cm
<br>@Temperature 400 °C
0.000132 ohm-cm
<br>@Temperature 752 °F
0.000134 ohm-cm
<br>@Temperature 500 °C
0.000134 ohm-cm
<br>@Temperature 932 °F
0.000135 ohm-cm
<br>@Temperature 600 °C
0.000135 ohm-cm
<br>@Temperature 1110 °F
Processing Properties Metric English Comments
Annealing Temperature 1135 - 1150 °C
2075 - 2100 °F
followed by rapid air-cooling or water quenching
Descriptive Properties Value Comments
Thermal Diffusivity (cm2/s) at 100°C
at 200°C
at 25°C
at 300°C
at 400°C
at 500°C
at 600°C
Copyright © lookpolymers.com All Rights Reserved