Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

DuPont Performance Polymers Zytel® FR7026V0F BK001 Nylon 66  (Unverified Data**)

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, Unreinforced, Flame Retardant
Manufacturer DuPont Performance Polymers
Trade Name Zytel®
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF DuPont Performance Polymers Zytel® FR7026V0F BK001 Nylon 66  (Unverified Data**).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Zytel® FR7026V0F BK001 is a flame retardant heat stabilized polyamide 66 resin for injection molding. It does not contain elemental phosphorous, halogens or heavy metals.Information provided by DuPont Performance Polymers
Physical Properties Metric English Comments
Density 1.16 g/cc
0.0419 lb/in³
DAM; ISO 1183
Linear Mold Shrinkage, Flow 0.0090 cm/cm
<br>@Thickness 2.00 mm
0.0090 in/in
<br>@Thickness 0.0787 in
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.010 cm/cm
<br>@Thickness 2.00 mm
0.010 in/in
<br>@Thickness 0.0787 in
DAM; ISO 294-4
Mechanical Properties Metric English Comments
Tensile Strength 70.0 MPa
<br>@Temperature 23.0 °C
10200 psi
<br>@Temperature 73.4 °F
DAM; ISO 527
Tensile Stress 1.14 MPa
<br>@Strain 0.100 %,<br> Temperature 80.0 °C
165 psi
<br>@Strain 0.100 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
2.95 MPa
<br>@Strain 0.200 %,<br> Temperature 80.0 °C
428 psi
<br>@Strain 0.200 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
3.10 MPa
<br>@Strain 0.100 %,<br> Temperature 60.0 °C
450 psi
<br>@Strain 0.100 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
3.69 MPa
<br>@Strain 0.100 %,<br> Temperature 23.0 °C
535 psi
<br>@Strain 0.100 %,<br> Temperature 73.4 °F
DAM; ISO 11403-1/-2
4.17 MPa
<br>@Strain 0.100 %,<br> Temperature -40.0 °C
605 psi
<br>@Strain 0.100 %,<br> Temperature -40.0 °F
DAM; ISO 11403-1/-2
4.23 MPa
<br>@Strain 0.100 %,<br> Temperature 0.000 °C
614 psi
<br>@Strain 0.100 %,<br> Temperature 32.0 °F
DAM; ISO 11403-1/-2
4.26 MPa
<br>@Strain 0.300 %,<br> Temperature 80.0 °C
618 psi
<br>@Strain 0.300 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
4.67 MPa
<br>@Strain 0.200 %,<br> Temperature 60.0 °C
677 psi
<br>@Strain 0.200 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
5.45 MPa
<br>@Strain 0.400 %,<br> Temperature 80.0 °C
790 psi
<br>@Strain 0.400 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
6.47 MPa
<br>@Strain 0.500 %,<br> Temperature 80.0 °C
938 psi
<br>@Strain 0.500 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
6.64 MPa
<br>@Strain 0.300 %,<br> Temperature 60.0 °C
963 psi
<br>@Strain 0.300 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
7.37 MPa
<br>@Strain 0.200 %,<br> Temperature 23.0 °C
1070 psi
<br>@Strain 0.200 %,<br> Temperature 73.4 °F
DAM; ISO 11403-1/-2
7.61 MPa
<br>@Strain 0.200 %,<br> Temperature -40.0 °C
1100 psi
<br>@Strain 0.200 %,<br> Temperature -40.0 °F
DAM; ISO 11403-1/-2
7.80 MPa
<br>@Strain 0.600 %,<br> Temperature 80.0 °C
1130 psi
<br>@Strain 0.600 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
7.97 MPa
<br>@Strain 0.200 %,<br> Temperature 0.000 °C
1160 psi
<br>@Strain 0.200 %,<br> Temperature 32.0 °F
DAM; ISO 11403-1/-2
8.44 MPa
<br>@Strain 0.400 %,<br> Temperature 60.0 °C
1220 psi
<br>@Strain 0.400 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
9.22 MPa
<br>@Strain 0.700 %,<br> Temperature 80.0 °C
1340 psi
<br>@Strain 0.700 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
10.28 MPa
<br>@Strain 0.800 %,<br> Temperature 80.0 °C
1491 psi
<br>@Strain 0.800 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
10.52 MPa
<br>@Strain 0.500 %,<br> Temperature 60.0 °C
1526 psi
<br>@Strain 0.500 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
11.05 MPa
<br>@Strain 0.300 %,<br> Temperature 23.0 °C
1603 psi
<br>@Strain 0.300 %,<br> Temperature 73.4 °F
DAM; ISO 11403-1/-2
11.12 MPa
<br>@Strain 0.900 %,<br> Temperature 80.0 °C
1613 psi
<br>@Strain 0.900 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
11.26 MPa
<br>@Strain 0.300 %,<br> Temperature -40.0 °C
1633 psi
<br>@Strain 0.300 %,<br> Temperature -40.0 °F
DAM; ISO 11403-1/-2
11.74 MPa
<br>@Strain 1.00 %,<br> Temperature 80.0 °C
1703 psi
<br>@Strain 1.00 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
11.9 MPa
<br>@Strain 0.300 %,<br> Temperature 0.000 °C
1730 psi
<br>@Strain 0.300 %,<br> Temperature 32.0 °F
DAM; ISO 11403-1/-2
12.07 MPa
<br>@Strain 0.600 %,<br> Temperature 60.0 °C
1751 psi
<br>@Strain 0.600 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
12.33 MPa
<br>@Strain 1.10 %,<br> Temperature 80.0 °C
1788 psi
<br>@Strain 1.10 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
13.06 MPa
<br>@Strain 1.20 %,<br> Temperature 80.0 °C
1894 psi
<br>@Strain 1.20 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
13.77 MPa
<br>@Strain 1.30 %,<br> Temperature 80.0 °C
1997 psi
<br>@Strain 1.30 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
13.85 MPa
<br>@Strain 0.700 %,<br> Temperature 60.0 °C
2009 psi
<br>@Strain 0.700 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
14.05 MPa
<br>@Strain 0.400 %,<br> Temperature 23.0 °C
2038 psi
<br>@Strain 0.400 %,<br> Temperature 73.4 °F
DAM; ISO 11403-1/-2
14.44 MPa
<br>@Strain 1.40 %,<br> Temperature 80.0 °C
2094 psi
<br>@Strain 1.40 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
15.07 MPa
<br>@Strain 1.50 %,<br> Temperature 80.0 °C
2186 psi
<br>@Strain 1.50 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
15.14 MPa
<br>@Strain 0.400 %,<br> Temperature -40.0 °C
2196 psi
<br>@Strain 0.400 %,<br> Temperature -40.0 °F
DAM; ISO 11403-1/-2
15.71 MPa
<br>@Strain 1.60 %,<br> Temperature 80.0 °C
2279 psi
<br>@Strain 1.60 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
15.74 MPa
<br>@Strain 0.400 %,<br> Temperature 0.000 °C
2283 psi
<br>@Strain 0.400 %,<br> Temperature 32.0 °F
DAM; ISO 11403-1/-2
15.96 MPa
<br>@Strain 0.800 %,<br> Temperature 60.0 °C
2315 psi
<br>@Strain 0.800 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
16.15 MPa
<br>@Strain 1.70 %,<br> Temperature 80.0 °C
2342 psi
<br>@Strain 1.70 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
16.56 MPa
<br>@Strain 1.80 %,<br> Temperature 80.0 °C
2402 psi
<br>@Strain 1.80 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
17.15 MPa
<br>@Strain 1.90 %,<br> Temperature 80.0 °C
2487 psi
<br>@Strain 1.90 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
17.65 MPa
<br>@Strain 2.00 %,<br> Temperature 80.0 °C
2560 psi
<br>@Strain 2.00 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
18.07 MPa
<br>@Strain 0.900 %,<br> Temperature 60.0 °C
2621 psi
<br>@Strain 0.900 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
18.18 MPa
<br>@Strain 2.10 %,<br> Temperature 80.0 °C
2637 psi
<br>@Strain 2.10 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
18.29 MPa
<br>@Strain 0.500 %,<br> Temperature 23.0 °C
2653 psi
<br>@Strain 0.500 %,<br> Temperature 73.4 °F
DAM; ISO 11403-1/-2
18.52 MPa
<br>@Strain 2.20 %,<br> Temperature 80.0 °C
2686 psi
<br>@Strain 2.20 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
18.91 MPa
<br>@Strain 2.30 %,<br> Temperature 80.0 °C
2743 psi
<br>@Strain 2.30 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
19.07 MPa
<br>@Strain 0.500 %,<br> Temperature -40.0 °C
2766 psi
<br>@Strain 0.500 %,<br> Temperature -40.0 °F
DAM; ISO 11403-1/-2
19.37 MPa
<br>@Strain 2.40 %,<br> Temperature 80.0 °C
2809 psi
<br>@Strain 2.40 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
19.49 MPa
<br>@Strain 0.500 %,<br> Temperature 0.000 °C
2827 psi
<br>@Strain 0.500 %,<br> Temperature 32.0 °F
DAM; ISO 11403-1/-2
19.62 MPa
<br>@Strain 1.00 %,<br> Temperature 60.0 °C
2846 psi
<br>@Strain 1.00 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
19.84 MPa
<br>@Strain 2.50 %,<br> Temperature 80.0 °C
2878 psi
<br>@Strain 2.50 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
20.25 MPa
<br>@Strain 2.60 %,<br> Temperature 80.0 °C
2937 psi
<br>@Strain 2.60 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
20.62 MPa
<br>@Strain 2.70 %,<br> Temperature 80.0 °C
2991 psi
<br>@Strain 2.70 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
20.87 MPa
<br>@Strain 2.80 %,<br> Temperature 80.0 °C
3027 psi
<br>@Strain 2.80 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
21.17 MPa
<br>@Strain 1.10 %,<br> Temperature 60.0 °C
3070 psi
<br>@Strain 1.10 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
21.34 MPa
<br>@Strain 2.90 %,<br> Temperature 80.0 °C
3095 psi
<br>@Strain 2.90 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
21.7 MPa
<br>@Strain 3.00 %,<br> Temperature 80.0 °C
3150 psi
<br>@Strain 3.00 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
21.89 MPa
<br>@Strain 0.600 %,<br> Temperature 23.0 °C
3175 psi
<br>@Strain 0.600 %,<br> Temperature 73.4 °F
DAM; ISO 11403-1/-2
22.04 MPa
<br>@Strain 3.10 %,<br> Temperature 80.0 °C
3197 psi
<br>@Strain 3.10 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
22.3 MPa
<br>@Strain 3.20 %,<br> Temperature 80.0 °C
3230 psi
<br>@Strain 3.20 %,<br> Temperature 176 °F
DAM; ISO 11403-1/-2
22.55 MPa
<br>@Strain 1.20 %,<br> Temperature 60.0 °C
3271 psi
<br>@Strain 1.20 %,<br> Temperature 140 °F
DAM; ISO 11403-1/-2
Copyright © lookpolymers.com All Rights Reserved