| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.03 g/cc | 0.0372 lb/in³ | |
| 1.21 g/cc | 0.0437 lb/in³ | DAM; ISO 1183 | |
| Water Absorption | 6.5 % @Thickness 2.00 mm |
6.5 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Moisture Absorption | 2.20 % @Thickness 2.00 mm |
2.20 % @Thickness 0.0787 in |
DAM; Sim. to ISO 62 |
| Viscosity | 54330 cP @Shear Rate 5000 1/s, Temperature 305 °C |
54330 cP @Shear Rate 5000 1/s, Temperature 581 °F |
ISO 11403-1 -2 |
| 61050 cP @Shear Rate 5000 1/s, Temperature 295 °C |
61050 cP @Shear Rate 5000 1/s, Temperature 563 °F |
ISO 11403-1 -2 | |
| 69096 cP @Shear Rate 5000 1/s, Temperature 285 °C |
69096 cP @Shear Rate 5000 1/s, Temperature 545 °F |
ISO 11403-1 -2 | |
| 157900 cP @Shear Rate 500 1/s, Temperature 305 °C |
157900 cP @Shear Rate 500 1/s, Temperature 581 °F |
ISO 11403-1 -2 | |
| 183700 cP @Shear Rate 500 1/s, Temperature 295 °C |
183700 cP @Shear Rate 500 1/s, Temperature 563 °F |
ISO 11403-1 -2 | |
| 214400 cP @Shear Rate 500 1/s, Temperature 285 °C |
214400 cP @Shear Rate 500 1/s, Temperature 545 °F |
ISO 11403-1 -2 | |
| Viscosity Test | 150 cm³/g | 150 cm³/g | DAM; ISO 307 1157 1628 |
| Linear Mold Shrinkage, Flow | 0.0040 cm/cm | 0.0040 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.0080 cm/cm | 0.0080 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 74 | 74 | 50%RH; ISO 2039-2 |
| 90 | 90 | DAM; ISO 2039-2 | |
| Hardness, Rockwell R | 110 | 110 | 50%RH; ISO 2039-2 |
| 120 | 120 | DAM; ISO 2039-2 | |
| Tensile Strength at Break | 67.0 MPa | 9720 psi | 50%RH; ISO 527-1/-2 |
| 118 MPa | 17100 psi | DAM; ISO 527-1/-2 | |
| Tensile Stress | 4.65 MPa @Strain 0.240 %, Temperature 150 °C |
674 psi @Strain 0.240 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 |
| 4.70 MPa @Strain 0.260 %, Temperature 150 °C |
682 psi @Strain 0.260 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 7.91 MPa @Strain 0.330 %, Temperature 90.0 °C |
1150 psi @Strain 0.330 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 8.28 MPa @Strain 0.360 %, Temperature 90.0 °C |
1200 psi @Strain 0.360 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 12.34 MPa @Strain 0.310 %, Temperature 23.0 °C |
1790 psi @Strain 0.310 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 13.93 MPa @Strain 0.890 %, Temperature 150 °C |
2020 psi @Strain 0.890 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 16.71 MPa @Strain 0.540 %, Temperature 40.0 °C |
2424 psi @Strain 0.540 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 16.91 MPa @Strain 0.260 %, Temperature -40.0 °C |
2453 psi @Strain 0.260 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 18.45 MPa @Strain 1.10 %, Temperature 150 °C |
2676 psi @Strain 1.10 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 19.46 MPa @Strain 0.390 %, Temperature 40.0 °C |
2822 psi @Strain 0.390 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 20.7 MPa @Strain 1.03 %, Temperature 90.0 °C |
3000 psi @Strain 1.03 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 21.67 MPa @Strain 1.00 %, Temperature 90.0 °C |
3143 psi @Strain 1.00 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 23.83 MPa @Strain 1.80 %, Temperature 150 °C |
3456 psi @Strain 1.80 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 29.84 MPa @Strain 2.07 %, Temperature 150 °C |
4328 psi @Strain 2.07 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 31.46 MPa @Strain 3.05 %, Temperature 150 °C |
4563 psi @Strain 3.05 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 31.64 MPa @Strain 0.590 %, Temperature 0.000 °C |
4589 psi @Strain 0.590 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 33.43 MPa @Strain 0.570 %, Temperature -20.0 °C |
4849 psi @Strain 0.570 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 33.91 MPa @Strain 1.93 %, Temperature 90.0 °C |
4918 psi @Strain 1.93 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 35.36 MPa @Strain 1.30 %, Temperature 40.0 °C |
5129 psi @Strain 1.30 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 35.58 MPa @Strain 0.950 %, Temperature 23.0 °C |
5160 psi @Strain 0.950 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 36.72 MPa @Strain 1.91 %, Temperature 90.0 °C |
5326 psi @Strain 1.91 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 38.56 MPa @Strain 3.29 %, Temperature 150 °C |
5593 psi @Strain 3.29 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 38.75 MPa @Strain 0.680 %, Temperature -40.0 °C |
5620 psi @Strain 0.680 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 43.99 MPa @Strain 3.18 %, Temperature 90.0 °C |
6380 psi @Strain 3.18 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 50.05 MPa @Strain 2.98 %, Temperature 90.0 °C |
7259 psi @Strain 2.98 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 52.98 MPa @Strain 2.23 %, Temperature 40.0 °C |
7684 psi @Strain 2.23 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 56.61 MPa @Strain 1.13 %, Temperature 0.000 °C |
8211 psi @Strain 1.13 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 60.02 MPa @Strain 1.85 %, Temperature 23.0 °C |
8705 psi @Strain 1.85 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 60.26 MPa @Strain 1.30 %, Temperature 40.0 °C |
8740 psi @Strain 1.30 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 61.44 MPa @Strain 1.22 %, Temperature 23.0 °C |
8911 psi @Strain 1.22 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 65.97 MPa @Strain 3.47 %, Temperature 40.0 °C |
9568 psi @Strain 3.47 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 75.79 MPa @Strain 1.42 %, Temperature 0.000 °C |
10990 psi @Strain 1.42 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 78.35 MPa @Strain 1.44 %, Temperature -40.0 °C |
11360 psi @Strain 1.44 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 | |
| 79.16 MPa @Strain 1.47 %, Temperature -20.0 °C |
11480 psi @Strain 1.47 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 80.24 MPa @Strain 2.97 %, Temperature 23.0 °C |
11640 psi @Strain 2.97 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 81.54 MPa @Strain 1.80 %, Temperature 0.000 °C |
11830 psi @Strain 1.80 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 89.54 MPa @Strain 2.23 %, Temperature 40.0 °C |
12990 psi @Strain 2.23 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 90.0 MPa @Strain 1.73 %, Temperature -20.0 °C |
13100 psi @Strain 1.73 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 92.9 MPa @Strain 2.00 %, Temperature 23.0 °C |
13500 psi @Strain 2.00 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 106.48 MPa @Strain 2.83 %, Temperature 0.000 °C |
15444 psi @Strain 2.83 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 106.92 MPa @Strain 4.62 %, Temperature 40.0 °C |
15507 psi @Strain 4.62 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 107.91 MPa @Strain 2.01 %, Temperature -40.0 °C |
15651 psi @Strain 2.01 %, Temperature -40.0 °F |
50%RH; ISO 11403-1 -2 | |
| 118.14 MPa @Strain 2.58 %, Temperature -20.0 °C |
17135 psi @Strain 2.58 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 118.3 MPa @Strain 3.01 %, Temperature 23.0 °C |
17160 psi @Strain 3.01 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 121.75 MPa @Strain 2.62 %, Temperature 0.000 °C |
17658 psi @Strain 2.62 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 126.15 MPa @Strain 2.59 %, Temperature -20.0 °C |
18297 psi @Strain 2.59 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 129.88 MPa @Strain 2.64 %, Temperature -40.0 °C |
18838 psi @Strain 2.64 %, Temperature -40.0 °F |
DAM; ISO 11403-1 -2 |