| Category | Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, 30% Glass Fiber Filled |
| Manufacturer | |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® 73G30T NC010 Nylon 6
(Unverified Data**).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.34 g/cc | 0.0484 lb/in³ | DAM; ISO 1183 |
| Filler Content | 30 % | 30 % | DAM |
| Water Absorption | 1.8 % @Temperature 23.0 °C |
1.8 % @Temperature 73.4 °F |
Equilibrium 50%RH; DAM; ISO 62, Similar to |
| 6.2 % @Temperature 23.0 °C |
6.2 % @Temperature 73.4 °F |
Saturation, immersed; DAM; ISO 62, Similar to | |
| Linear Mold Shrinkage, Flow | 0.0020 cm/cm @Thickness 2.00 mm |
0.0020 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Linear Mold Shrinkage, Transverse | 0.010 cm/cm @Thickness 2.00 mm |
0.010 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 110 MPa @Temperature 23.0 °C |
16000 psi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 170 MPa @Temperature 23.0 °C |
24700 psi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Elongation at Break | 3.0 % @Temperature 23.0 °C |
3.0 % @Temperature 73.4 °F |
DAM; ISO 527 |
| 6.0 % @Temperature 23.0 °C |
6.0 % @Temperature 73.4 °F |
50%RH; ISO 527 | |
| Tensile Modulus | 5.70 GPa @Temperature 23.0 °C |
827 ksi @Temperature 73.4 °F |
50%RH; ISO 527 |
| 9.10 GPa @Temperature 23.0 °C |
1320 ksi @Temperature 73.4 °F |
DAM; ISO 527 | |
| Flexural Modulus | 5.70 GPa @Temperature 23.0 °C |
827 ksi @Temperature 73.4 °F |
50%RH; ISO 178 |
| 9.00 GPa @Temperature 23.0 °C |
1310 ksi @Temperature 73.4 °F |
DAM; ISO 178 | |
| Shear Modulus | 0.00100 GPa @Temperature 228 °C |
0.145 ksi @Temperature 442 °F |
DAM; ISO 6721 |
| 0.0460 GPa @Temperature 224 °C |
6.67 ksi @Temperature 435 °F |
DAM; ISO 6721 | |
| 0.122 GPa @Temperature 220 °C |
17.7 ksi @Temperature 428 °F |
DAM; ISO 6721 | |
| 0.199 GPa @Temperature 216 °C |
28.9 ksi @Temperature 421 °F |
DAM; ISO 6721 | |
| 0.232 GPa @Temperature 214 °C |
33.6 ksi @Temperature 417 °F |
DAM; ISO 6721 | |
| 0.290 GPa @Temperature 210 °C |
42.1 ksi @Temperature 410 °F |
DAM; ISO 6721 | |
| 0.347 GPa @Temperature 204 °C |
50.3 ksi @Temperature 399 °F |
DAM; ISO 6721 | |
| 0.383 GPa @Temperature 200 °C |
55.6 ksi @Temperature 392 °F |
DAM; ISO 6721 | |
| 0.445 GPa @Temperature 190 °C |
64.5 ksi @Temperature 374 °F |
DAM; ISO 6721 | |
| 0.482 GPa @Temperature 180 °C |
69.9 ksi @Temperature 356 °F |
DAM; ISO 6721 | |
| 0.506 GPa @Temperature 170 °C |
73.4 ksi @Temperature 338 °F |
DAM; ISO 6721 | |
| 0.524 GPa @Temperature 160 °C |
76.0 ksi @Temperature 320 °F |
DAM; ISO 6721 | |
| 0.537 GPa @Temperature 150 °C |
77.9 ksi @Temperature 302 °F |
DAM; ISO 6721 | |
| 0.548 GPa @Temperature 140 °C |
79.5 ksi @Temperature 284 °F |
DAM; ISO 6721 | |
| 0.557 GPa @Temperature 130 °C |
80.8 ksi @Temperature 266 °F |
DAM; ISO 6721 | |
| 0.569 GPa @Temperature 118 °C |
82.5 ksi @Temperature 244 °F |
DAM; ISO 6721 | |
| 0.578 GPa @Temperature 110 °C |
83.8 ksi @Temperature 230 °F |
DAM; ISO 6721 | |
| 0.593 GPa @Temperature 100 °C |
86.0 ksi @Temperature 212 °F |
DAM; ISO 6721 | |
| 0.614 GPa @Temperature 90.0 °C |
89.1 ksi @Temperature 194 °F |
DAM; ISO 6721 | |
| 0.650 GPa @Temperature 80.0 °C |
94.3 ksi @Temperature 176 °F |
DAM; ISO 6721 | |
| 0.712 GPa @Temperature 70.0 °C |
103 ksi @Temperature 158 °F |
DAM; ISO 6721 | |
| 0.834 GPa @Temperature 60.0 °C |
121 ksi @Temperature 140 °F |
DAM; ISO 6721 | |
| 1.111 GPa @Temperature 50.0 °C |
161.1 ksi @Temperature 122 °F |
DAM; ISO 6721 | |
| 1.443 GPa @Temperature 40.0 °C |
209.3 ksi @Temperature 104 °F |
DAM; ISO 6721 | |
| 1.573 GPa @Temperature 30.0 °C |
228.1 ksi @Temperature 86.0 °F |
DAM; ISO 6721 | |
| 1.656 GPa @Temperature 20.0 °C |
240.2 ksi @Temperature 68.0 °F |
DAM; ISO 6721 | |
| 1.716 GPa @Temperature 10.0 °C |
248.9 ksi @Temperature 50.0 °F |
DAM; ISO 6721 | |
| 1.751 GPa @Temperature 0.000 °C |
254.0 ksi @Temperature 32.0 °F |
DAM; ISO 6721 | |
| 1.769 GPa @Temperature -10.0 °C |
256.6 ksi @Temperature 14.0 °F |
DAM; ISO 6721 | |
| 1.783 GPa @Temperature -20.0 °C |
258.6 ksi @Temperature -4.00 °F |
DAM; ISO 6721 | |
| 1.805 GPa @Temperature -30.0 °C |
261.8 ksi @Temperature -22.0 °F |
DAM; ISO 6721 | |
| 1.847 GPa @Temperature -40.0 °C |
267.9 ksi @Temperature -40.0 °F |
DAM; ISO 6721 | |
| 1.93 GPa @Temperature -50.0 °C |
280 ksi @Temperature -58.0 °F |
DAM; ISO 6721 | |
| Izod Impact, Notched (ISO) | 12.0 kJ/m² @Temperature -30.0 °C |
5.71 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 180/1A |
| 12.0 kJ/m² @Temperature -30.0 °C |
5.71 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 180/1A | |
| 17.0 kJ/m² @Temperature 23.0 °C |
8.09 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 180/1A | |
| 24.0 kJ/m² @Temperature 23.0 °C |
11.4 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 180/1A | |
| Izod Impact, Unnotched (ISO) | 80.0 kJ/m² @Temperature 23.0 °C |
38.1 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 180/1U |
| 80.0 kJ/m² @Temperature 23.0 °C |
38.1 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 180/1U | |
| Charpy Impact Unnotched | 9.40 J/cm² @Temperature -30.0 °C |
44.7 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eU |
| 10.0 J/cm² @Temperature -30.0 °C |
47.6 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eU | |
| 10.0 J/cm² @Temperature 23.0 °C |
47.6 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eU | |
| 10.0 J/cm² @Temperature 23.0 °C |
47.6 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eU | |
| Charpy Impact, Notched | 1.20 J/cm² @Temperature -30.0 °C |
5.71 ft-lb/in² @Temperature -22.0 °F |
50%RH; ISO 179/1eA |
| 1.30 J/cm² @Temperature -30.0 °C |
6.19 ft-lb/in² @Temperature -22.0 °F |
DAM; ISO 179/1eA | |
| 2.00 J/cm² @Temperature 23.0 °C |
9.52 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 179/1eA | |
| 2.50 J/cm² @Temperature 23.0 °C |
11.9 ft-lb/in² @Temperature 73.4 °F |
50%RH; ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 500 µm/m-°C @Temperature 23.0 - 55.0 °C |
278 µin/in-°F @Temperature 73.4 - 131 °F |
DAM; ASTM E 831 |
| 500 µm/m-°C @Temperature 23.0 - 55.0 °C |
278 µin/in-°F @Temperature 73.4 - 131 °F |
DAM; ISO 11359-1/-2 | |
| CTE, linear, Transverse to Flow | 120 µm/m-°C @Temperature 23.0 - 55.0 °C |
66.7 µin/in-°F @Temperature 73.4 - 131 °F |
DAM; ASTM E 831 |
| 120 µm/m-°C @Temperature 23.0 - 55.0 °C |
66.7 µin/in-°F @Temperature 73.4 - 131 °F |
DAM; ISO 11359-1/-2 |