Physical Properties | Metric | English | Comments |
---|---|---|---|
Density | 1.42 g/cc | 0.0513 lb/in³ | ISO 1183 |
Viscosity | 94957 cP @Shear Rate 5000 1/s, Temperature 230 °C |
94957 cP @Shear Rate 5000 1/s, Temperature 446 °F |
ISO 11403-1 -2 |
99460 cP @Shear Rate 5000 1/s, Temperature 215 °C |
99460 cP @Shear Rate 5000 1/s, Temperature 419 °F |
ISO 11403-1 -2 | |
106400 cP @Shear Rate 5000 1/s, Temperature 200 °C |
106400 cP @Shear Rate 5000 1/s, Temperature 392 °F |
ISO 11403-1 -2 | |
244860 cP @Shear Rate 500 1/s, Temperature 230 °C |
244860 cP @Shear Rate 500 1/s, Temperature 446 °F |
ISO 11403-1 -2 | |
303800 cP @Shear Rate 500 1/s, Temperature 215 °C |
303800 cP @Shear Rate 500 1/s, Temperature 419 °F |
ISO 11403-1 -2 | |
349300 cP @Shear Rate 500 1/s, Temperature 200 °C |
349300 cP @Shear Rate 500 1/s, Temperature 392 °F |
ISO 11403-1 -2 | |
Linear Mold Shrinkage, Flow | 0.020 cm/cm | 0.020 in/in | ISO 294-4 2577 |
Linear Mold Shrinkage, Transverse | 0.019 cm/cm | 0.019 in/in | ISO 294-4 2577 |
Melt Flow | 12 g/10 min @Load 2.16 kg, Temperature 190 °C |
12 g/10 min @Load 4.76 lb, Temperature 374 °F |
cm³/10min; ISO 1133 |
14 g/10 min @Load 2.16 kg, Temperature 190 °C |
14 g/10 min @Load 4.76 lb, Temperature 374 °F |
ISO 1133 |
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Hardness, Rockwell M | 93 | 93 | ISO 2039-2 |
Hardness, Rockwell R | 122 | 122 | ISO 2039-2 |
Tensile Stress | 5.60 MPa @Strain 0.400 %, Temperature 90.0 °C |
812 psi @Strain 0.400 %, Temperature 194 °F |
ISO 11403-1 -2 |
19.5 MPa @Strain 0.600 %, Temperature 23.0 °C |
2830 psi @Strain 0.600 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
20.1 MPa @Strain 1.90 %, Temperature 90.0 °C |
2920 psi @Strain 1.90 %, Temperature 194 °F |
ISO 11403-1 -2 | |
26.6 MPa @Strain 0.700 %, Temperature 0.000 °C |
3860 psi @Strain 0.700 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
28.1 MPa @Strain 3.30 %, Temperature 90.0 °C |
4080 psi @Strain 3.30 %, Temperature 194 °F |
ISO 11403-1 -2 | |
33.0 MPa @Strain 4.80 %, Temperature 90.0 °C |
4790 psi @Strain 4.80 %, Temperature 194 °F |
ISO 11403-1 -2 | |
33.0 MPa @Strain 0.700 %, Temperature -40.0 °C |
4790 psi @Strain 0.700 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
52.3 MPa @Strain 2.60 %, Temperature 23.0 °C |
7590 psi @Strain 2.60 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
61.9 MPa @Strain 4.50 %, Temperature 23.0 °C |
8980 psi @Strain 4.50 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
65.7 MPa @Strain 7.00 %, Temperature 23.0 °C |
9530 psi @Strain 7.00 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
68.9 MPa @Strain 3.00 %, Temperature 0.000 °C |
9990 psi @Strain 3.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
79.6 MPa @Strain 5.00 %, Temperature 0.000 °C |
11500 psi @Strain 5.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
83.7 MPa @Strain 8.00 %, Temperature 0.000 °C |
12100 psi @Strain 8.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
88.2 MPa @Strain 2.90 %, Temperature -40.0 °C |
12800 psi @Strain 2.90 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
95.7 MPa @Strain 5.00 %, Temperature -40.0 °C |
13900 psi @Strain 5.00 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
98.2 MPa @Strain 8.00 %, Temperature -40.0 °C |
14200 psi @Strain 8.00 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
Tensile Strength, Yield | 73.0 MPa | 10600 psi | ISO 527-1/-2 |
Elongation at Break | 22 % | 22 % | Nominal; ISO 527-1/-2 |
Elongation at Yield | 15 % | 15 % | ISO 527-1/-2 |
Tensile Modulus | 3.25 GPa | 471 ksi | ISO 527-1/-2 |
Flexural Modulus | 3.05 GPa | 442 ksi | ISO 178 |
Secant Modulus | 0.698 GPa @Strain 14.2 %, Temperature -40.0 °C |
101 ksi @Strain 14.2 %, Temperature -40.0 °F |
ISO 11403-1 -2 |
0.741 GPa @Strain 9.00 %, Temperature 23.0 °C |
107 ksi @Strain 9.00 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
0.845 GPa @Strain 10.0 %, Temperature 0.000 °C |
123 ksi @Strain 10.0 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
0.986 GPa @Strain 10.0 %, Temperature -40.0 °C |
143 ksi @Strain 10.0 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
1.262 GPa @Strain 5.00 %, Temperature 23.0 °C |
183.0 ksi @Strain 5.00 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
1.36 GPa @Strain 6.00 %, Temperature 0.000 °C |
197 ksi @Strain 6.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
1.62 GPa @Strain 6.00 %, Temperature -40.0 °C |
234 ksi @Strain 6.00 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
2.01 GPa @Strain 2.60 %, Temperature 23.0 °C |
292 ksi @Strain 2.60 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
2.30 GPa @Strain 3.00 %, Temperature 0.000 °C |
333 ksi @Strain 3.00 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
3.04 GPa @Strain 2.90 %, Temperature -40.0 °C |
441 ksi @Strain 2.90 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
3.25 GPa @Strain 0.600 %, Temperature 23.0 °C |
471 ksi @Strain 0.600 %, Temperature 73.4 °F |
ISO 11403-1 -2 | |
3.80 GPa @Strain 0.700 %, Temperature 0.000 °C |
551 ksi @Strain 0.700 %, Temperature 32.0 °F |
ISO 11403-1 -2 | |
4.71 GPa @Strain 0.700 %, Temperature -40.0 °C |
684 ksi @Strain 0.700 %, Temperature -40.0 °F |
ISO 11403-1 -2 | |
Charpy Impact Unnotched | 30.0 J/cm² | 143 ft-lb/in² | ISO 179/1eU |
25.0 J/cm² @Temperature -30.0 °C |
119 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eU | |
Charpy Impact, Notched | 0.950 J/cm² | 4.52 ft-lb/in² | ISO 179/1eA |
0.900 J/cm² @Temperature -30.0 °C |
4.28 ft-lb/in² @Temperature -22.0 °F |
ISO 179/1eA |
Thermal Properties | Metric | English | Comments |
---|---|---|---|
CTE, linear, Parallel to Flow | 110 µm/m-°C | 61.1 µin/in-°F | ISO 11359-1/-2 |
100 µm/m-°C @Temperature -40.0 - 23.0 °C |
55.6 µin/in-°F @Temperature -40.0 - 73.4 °F |
ISO 11359-1/-2 | |
CTE, linear, Transverse to Flow | 110 µm/m-°C | 61.1 µin/in-°F | ISO 11359-1/-2 |
90.0 µm/m-°C @Temperature -40.0 - 23.0 °C |
50.0 µin/in-°F @Temperature -40.0 - 73.4 °F |
ISO 11359-1/-2 | |
Melting Point | 178 °C | 352 °F | 10°C/min; ISO 11357-1/-3 |
Deflection Temperature at 0.46 MPa (66 psi) | 158 °C | 316 °F | ISO 75-1/-2 |
Deflection Temperature at 1.8 MPa (264 psi) | 93.0 °C | 199 °F | ISO 75-1/-2 |
Electrical Properties | Metric | English | Comments |
---|---|---|---|
Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm | IEC 60093 |
Surface Resistance | 3.00e+14 ohm | 3.00e+14 ohm | IEC 60093 |
Dielectric Constant | 3.8 @Frequency 100 Hz |
3.8 @Frequency 100 Hz |
IEC 60250 |
3.8 @Frequency 1.00e+6 Hz |
3.8 @Frequency 1.00e+6 Hz |
IEC 60250 | |
Dielectric Strength | 47.0 kV/mm | 1190 kV/in | IEC 60243-1 |
Dissipation Factor | 0.0010 @Frequency 100 Hz |
0.0010 @Frequency 100 Hz |
IEC 60250 |
0.0055 @Frequency 1.00e+6 Hz |
0.0055 @Frequency 1.00e+6 Hz |
IEC 60250 | |
Comparative Tracking Index | 600 V | 600 V | IEC 60112 |
Descriptive Properties | Value | Comments |
---|---|---|
Additives | Release agent | |
Delivery Form | Pellets |