Category Metal , Ferrous Metal , Tool Steel , Air-Hardening Steel
Manufacturer Crucible Steel
Trade Name CSM®
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Crucible Steel CSM® 6 Tool Steel, AISI A6.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
CSM 6 is an air hardening tool steel offering moderate wear resistance and toughness. It may be hardened from a low hardening temperature for easy heat treatment.Information provided by Crucible Industries
Physical Properties Metric English Comments
Density 7.83 g/cc
0.283 lb/in³
Mechanical Properties Metric English Comments
Hardness, Brinell 217 - 248
217 - 248
Hardness, Rockwell C 48
<br>@Tempering Temp. 538 °C
48
<br>@Tempering Temp. 1000 °F
hardened at 1855°F then tempered
50
<br>@Tempering Temp. 482 °C
50
<br>@Tempering Temp. 900 °F
hardened at 1855°F then tempered
52
<br>@Tempering Temp. 427 °C
52
<br>@Tempering Temp. 800 °F
hardened at 1855°F then tempered
54
<br>@Tempering Temp. 371 °C
54
<br>@Tempering Temp. 700 °F
hardened at 1855°F then tempered
55
<br>@Tempering Temp. 316 °C
55
<br>@Tempering Temp. 600 °F
hardened at 1855°F then tempered
56
<br>@Tempering Temp. 260 °C
56
<br>@Tempering Temp. 500 °F
hardened at 1855°F then tempered
58
<br>@Tempering Temp. 204 °C
58
<br>@Tempering Temp. 400 °F
hardened at 1855°F then tempered
60
<br>@Tempering Temp. 149 °C
60
<br>@Tempering Temp. 300 °F
hardened at 1855°F then tempered
61
<br>@Tempering Temp. 93.3 °C
61
<br>@Tempering Temp. 200 °F
hardened at 1855°F then tempered
Modulus of Elasticity 207 GPa
30000 ksi
Charpy Impact 36.6 J
<br>@Tempering Temp. 149 °C
27.0 ft-lb
<br>@Tempering Temp. 300 °F
austenitizied at 1550°F then tempered; C-notch
59.7 J
<br>@Tempering Temp. 204 °C
44.0 ft-lb
<br>@Tempering Temp. 400 °F
austenitizied at 1550°F then tempered; C-notch
81.3 J
<br>@Tempering Temp. 260 °C
60.0 ft-lb
<br>@Tempering Temp. 500 °F
austenitizied at 1550°F then tempered; C-notch
90.8 J
<br>@Tempering Temp. 316 °C
67.0 ft-lb
<br>@Tempering Temp. 600 °F
austenitizied at 1550°F then tempered; C-notch
Thermal Properties Metric English Comments
CTE, linear 11.9 µm/m-°C
<br>@Temperature 20.0 - 93.3 °C
6.60 µin/in-°F
<br>@Temperature 68.0 - 200 °F
12.4 µm/m-°C
<br>@Temperature 20.0 - 204 °C
6.90 µin/in-°F
<br>@Temperature 68.0 - 400 °F
13.0 µm/m-°C
<br>@Temperature 20.0 - 316 °C
7.20 µin/in-°F
<br>@Temperature 68.0 - 600 °F
13.5 µm/m-°C
<br>@Temperature 20.0 - 427 °C
7.50 µin/in-°F
<br>@Temperature 68.0 - 800 °F
13.9 µm/m-°C
<br>@Temperature 20.0 - 538 °C
7.70 µin/in-°F
<br>@Temperature 68.0 - 1000 °F
Thermal Conductivity 2.59 - 2.74 W/m-K
18.0 - 19.0 BTU-in/hr-ft²-°F
Component Elements Properties Metric English Comments
Carbon, C 0.70 %
0.70 %
Chromium, Cr 1.0 %
1.0 %
Iron, Fe 94.65 %
94.65 %
as balance
Manganese, Mn 2.0 %
2.0 %
Molybdenum, Mo 1.35 %
1.35 %
Silicon, Si 0.30 %
0.30 %