Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Arkema Group Orgalloy® RS 66M25 Nylon 66 Alloy, 25% Mineral Filled (Conditioned)

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, 30% Mineral Filled
Manufacturer Arkema
Trade Name Orgalloy®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Arkema Group Orgalloy® RS 66M25 Nylon 66 Alloy, 25% Mineral Filled (Conditioned).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
RS 66 series, rigid polyamide 66 alloy: easy to process, chemical resistance (no known solvents) and low moisture absorption leading to stability of mechanical, electrical and dimensional properties.Mineral filled (25%) for injection molding of technical parts. Isotropy and low distortion, offers precisely dimensioned injection moldings.ISO data provided by the manufacturer, Arkema.
Physical Properties Metric English Comments
Density 1.23 g/cc
0.0444 lb/in³
Water Absorption 2.3 %
2.3 %
Moisture Absorption at Equilibrium 1.05 %
1.05 %
Humidity Absorption
Melt Flow 9.5 g/10 min

@Load 2.16 kg,
Temperature 275 °C
9.5 g/10 min

@Load 4.76 lb,
Temperature 527 °F
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 67.0 MPa
9720 psi
5 mm/min
Elongation at Break 3.1 %
3.1 %
5 mm/min
Tensile Modulus 5.50 GPa
798 ksi
1 mm/min
Charpy Impact, Notched 0.600 J/cm²
2.86 ft-lb/in²
0.400 J/cm²

@Temperature -30.0 °C
1.90 ft-lb/in²

@Temperature -22.0 °F
Thermal Properties Metric English Comments
Melting Point 255 °C
491 °F
10°C/min
Flammability, UL94 HB

@Thickness 1.60 mm
HB

@Thickness 0.0630 in
HB

@Thickness 3.20 mm
HB

@Thickness 0.126 in
Electrical Properties Metric English Comments
Comparative Tracking Index 600 V
600 V
Users viewing this material also viewed the following: