Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Techmer ES HiFill® PA6/6 GF33 HR HS BK 33% Glass Filled

Category Polymer , Thermoplastic , Nylon , Nylon 66 , Nylon 66, 30% Glass Fiber Filled , Nylon 66, Heat Stabilized
Manufacturer Techmer ES
Trade Name HiFill®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Techmer ES HiFill® PA6/6 GF33 HR HS BK 33% Glass Filled.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Availability: North AmericaForms: PelletsFiller/Reinforcement: Glass Fiber Reinforcement, 33% Filler by WeightAdditive: Heat StabilizerFeatures: Heat Stabilized and Hydrolysis Resistant Appearance: BlackInformation provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.37 g/cc
0.0495 lb/in³
ASTM D792
Water Absorption 0.55 %

@Time 86400 sec
0.55 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0040 cm/cm

@Thickness 3.17 mm
0.0040 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell R 121
121
ASTM D785
Tensile Strength, Yield 18.8 MPa
2730 psi
ASTM D638
Elongation at Break 4.0 %
4.0 %
ASTM D638
Flexural Strength 262 MPa
38000 psi
ASTM D790
Flexural Modulus 8.89 GPa
1290 ksi
ASTM D790
Izod Impact, Notched 1.07 J/cm

@Thickness 3.17 mm
2.00 ft-lb/in

@Thickness 0.125 in
ASTM D256
Izod Impact, Unnotched 9.61 J/cm

@Thickness 3.17 mm
18.0 ft-lb/in

@Thickness 0.125 in
ASTM D256
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 32.4 µm/m-°C
18.0 µin/in-°F
ASTM D696
Melting Point 255 °C
491 °F
Deflection Temperature at 0.46 MPa (66 psi) 260 °C
500 °F
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 254 °C
490 °F
Unannealed; ASTM D648
Flammability, UL94 HB
HB
Electrical Properties Metric English Comments
Volume Resistivity 5.00e+14 ohm-cm
5.00e+14 ohm-cm
ASTM D257
Dielectric Strength 18.9 kV/mm
480 kV/in
Method A (Short-Time); ASTM D149
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved