Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 3.0 PHR Di-Cup 40C Peroxide, Hardness 65A

Category Polymer , Thermoset , Polyester, TS , Polyurethane, TS , Thermoset Polyurethane, Elastomer, Unreinforced , Rubber or Thermoset Elastomer (TSE)
Manufacturer TSE Industries, Inc
Trade Name Millathane®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 3.0 PHR Di-Cup 40C Peroxide, Hardness 65A.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Millathane® 76 is a very suitable choice for use in products such as bushings, small copier rolls; automotive applications — bumpers, o-rings, hydraulic seals, belts, gaskets, solid tires — and many other high performance polyurethane applications. Millathane 76 can be vulcanized by sulfur or peroxide cured systems.Curing of Millathane®76 can easily be done with many types of peroxides. Millathane76 peroxide vulcanizates have superior compression set, greater heat stability, and are more resistant to reversion than sulfur cures.FormulationMillathane 76 100.0Stearic Acid 0.5N-220 Black20.0Di-Cup 40C 3.0All information provided by TSE Industries
Mechanical Properties Metric English Comments
Hardness, Shore A 65
65
Tensile Strength, Yield 29.19 MPa
4234 psi
Elongation at Yield 367 %
367 %
100% Modulus 0.00279 GPa
0.405 ksi
200% Modulus 0.009604 GPa
1.393 ksi
300% Modulus 0.02099 GPa
3.045 ksi
Tear Strength 58.3 kN/m
333 pli
Die C
Compression Set 22 %

@Temperature 100 °C,
Time 79200 sec
22 %

@Temperature 212 °F,
Time 22.0 hour
Processing Properties Metric English Comments
Cure Time 15.0 min

@Temperature 160 °C
0.250 hour

@Temperature 320 °F
Users viewing this material also viewed the following: