| Category | Ceramic , Glass |
| Manufacturer | Schott North America |
| Trade Name | |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Schott N-LAF2 Glass.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 4.30 g/cc | 0.155 lb/in³ |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Knoop Microhardness | 530 | 530 | .1/20 |
| Modulus of Elasticity | 94.0 GPa | 13600 ksi | |
| Poissons Ratio | 0.288 | 0.288 | |
| Shear Modulus | 36.0 GPa | 5220 ksi | calculated |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 8.10 µm/m-°C <br>@Temperature -30.0 - 70.0 °C |
4.50 µin/in-°F <br>@Temperature -22.0 - 158 °F |
|
| 9.10 µm/m-°C <br>@Temperature 20.0 - 300 °C |
5.06 µin/in-°F <br>@Temperature 68.0 - 572 °F |
||
| Specific Heat Capacity | 0.510 J/g-°C | 0.122 BTU/lb-°F | |
| Thermal Conductivity | 0.670 W/m-K | 4.65 BTU-in/hr-ft²-°F | |
| Transformation Temperature, Tg | 653 °C | 1210 °F |
| Optical Properties | Metric | English | Comments |
|---|---|---|---|
| Refractive Index | 1.74397 <br>@Wavelength 587.6 nm |
1.74397 <br>@Wavelength 587.6 nm |
n<sub>d</sub> |
| 1.74791 <br>@Wavelength 546.1 nm |
1.74791 <br>@Wavelength 546.1 nm |
n<sub>e</sub> | |
| Transmission, Visible | 83.1 % <br>@Thickness 10.0 mm,<br> Wavelength 380 nm |
83.1 % <br>@Thickness 0.394 in,<br> Wavelength 380 nm |
|
| 94.4 % <br>@Thickness 10.0 mm,<br> Wavelength 405 nm |
94.4 % <br>@Thickness 0.394 in,<br> Wavelength 405 nm |
||
| 98.5 % <br>@Thickness 10.0 mm,<br> Wavelength 460 nm |
98.5 % <br>@Thickness 0.394 in,<br> Wavelength 460 nm |
||
| 99.7 % <br>@Thickness 10.0 mm,<br> Wavelength 580 nm |
99.7 % <br>@Thickness 0.394 in,<br> Wavelength 580 nm |
||
| 99.8 % <br>@Thickness 10.0 mm,<br> Wavelength 700 nm |
99.8 % <br>@Thickness 0.394 in,<br> Wavelength 700 nm |
||
| IR Transmittance | 69.3 % <br>@Thickness 10.0 mm,<br> Wavelength 2500 nm |
69.3 % <br>@Thickness 0.394 in,<br> Wavelength 2500 nm |
|
| 99.6 % <br>@Thickness 10.0 mm,<br> Wavelength 1530 nm |
99.6 % <br>@Thickness 0.394 in,<br> Wavelength 1530 nm |
||
| UV Transmittance | 22.9 % <br>@Thickness 10.0 mm,<br> Wavelength 350 nm |
22.9 % <br>@Thickness 0.394 in,<br> Wavelength 350 nm |
|
| 62.6 % <br>@Thickness 10.0 mm,<br> Wavelength 365 nm |
62.6 % <br>@Thickness 0.394 in,<br> Wavelength 365 nm |
||
| 71.3 % <br>@Thickness 10.0 mm,<br> Wavelength 370 nm |
71.3 % <br>@Thickness 0.394 in,<br> Wavelength 370 nm |
| Chemical Properties | Metric | English | Comments |
|---|---|---|---|
| Acid Class, SR | 52.2 | 52.2 | |
| Alkali Class, AR | 1.0 | 1.0 | |
| Stain Resistance Class, FR | 3.0 | 3.0 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| B | 1 | |
| Climatic Resistance Test CR | 2 | |
| HG | 6 | |
| K (10-6mm2/N) | 1.42 | |
| Phosphate Resistance PR | 2.2 | |
| T1013.0 (°C) | 645 | |
| T107.6 (°C) | 742 |