| Category | Polymer , Thermoplastic , Elastomer, TPE , Polyester TPE , Polyester, TP |
| Manufacturer | DSM Engineering Plastics |
| Trade Name | Arnitel® |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DSM Arnitel® EL250 TPC-ET.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.08 g/cc | 0.0390 lb/in³ | ISO 1183 |
| Water Absorption | 0.80 % | 0.80 % | Sim. To ISO 62 |
| Melt Flow | 41 g/10 min @Load 2.16 kg, Temperature 230 °C |
41 g/10 min @Load 4.76 lb, Temperature 446 °F |
cm<sup>3</sup>/10min Melt Volume-flow Rate; ISO 1133 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore D | 25 @Time 3.00 sec |
25 @Time 0.000833 hour |
ISO 868 |
| Tensile Strength, Ultimate | 16.0 MPa | 2320 psi | ISO 527-1/-2 |
| Tensile Stress | 1.20 MPa @Strain 5.00 % |
174 psi @Strain 5.00 % |
ISO 527-1/-2 |
| 2.10 MPa @Strain 10.0 % |
305 psi @Strain 10.0 % |
ISO 527-1/-2 | |
| 4.40 MPa @Strain 50.0 % |
638 psi @Strain 50.0 % |
ISO 527-1/-2 | |
| 5.10 MPa @Strain 100 % |
740 psi @Strain 100 % |
ISO 527-1/-2 | |
| Elongation at Break | 900 % | 900 % | ISO 527-1/-2 |
| Tensile Modulus | 0.0250 GPa | 3.63 ksi | ISO 527-1/-2 |
| Izod Impact Resistance | NB @Temperature 23.0 °C |
NB @Temperature 73.4 °F |
ISO 180/1A |
| Charpy Impact, Notched | NB @Temperature 23.0 °C |
NB @Temperature 73.4 °F |
ISO 179/1eA |
| NB @Temperature -30.0 °C |
NB @Temperature -22.0 °F |
ISO 179/1eA |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 220 µm/m-°C | 122 µin/in-°F | ISO 11359-1/-2 |
| CTE, linear, Transverse to Flow | 220 µm/m-°C | 122 µin/in-°F | ISO 11359-1/-2 |
| Melting Point | 180 °C | 356 °F | 10°C/min; ISO 11357-1/-3 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 5.00e+14 ohm-cm | 5.00e+14 ohm-cm | IEC 60093 |