Crucible Steel REX® M2 S High Speed Steel

Category Metal , Ferrous Metal , Tool Steel
Manufacturer Crucible Steel
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Crucible Steel REX® M2 S High Speed Steel.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
REX M2 is a tungsten-molybdenum high speed steel which gives outstanding performance in all operations where a general purpose high speed steel is required. REX M2 has a wide hardening range, excellent toughness, with good wear and red hardness characteristics. REX M2S is the sulfur-bearing counterpart of REX M2. The sulfur addition provides good grindability and an improvement in machinability of 25 to 35 per cent over a comparable nonsulfurized grade.Information provided by Crucible Industries
Physical Properties Metric English Comments
Density 8.14 g/cc
0.294 lb/in³
Mechanical Properties Metric English Comments
Hardness, Brinell 217 - 255
217 - 255
Hardness, Rockwell C 57

@Tempering Temp. 649 °C
57

@Tempering Temp. 1200 °F
hardened at 2250°F then tempered
59

@Tempering Temp. 635.0 °C
59

@Tempering Temp. 1175 °F
hardened at 2250°F then tempered
60.9

@Tempering Temp. 621 °C
60.9

@Tempering Temp. 1150 °F
hardened at 2250°F then tempered
62.4

@Tempering Temp. 607.2 °C
62.4

@Tempering Temp. 1125 °F
hardened at 2250°F then tempered
64

@Tempering Temp. 593 °C
64

@Tempering Temp. 1100 °F
hardened at 2250°F then tempered
65

@Tempering Temp. 579.4 °C
65

@Tempering Temp. 1075 °F
hardened at 2250°F then tempered
66

@Tempering Temp. 524 °C
66

@Tempering Temp. 975 °F
hardened at 2250°F then tempered
66

@Tempering Temp. 566 °C
66

@Tempering Temp. 1050 °F
hardened at 2250°F then tempered
66.8

@Tempering Temp. 538 °C
66.8

@Tempering Temp. 1000 °F
hardened at 2250°F then tempered
66.8

@Tempering Temp. 551.7 °C
66.8

@Tempering Temp. 1025 °F
hardened at 2250°F then tempered
Modulus of Elasticity 207 GPa
30000 ksi
Thermal Properties Metric English Comments
CTE, linear 11.5 µm/m-°C

@Temperature 21.1 - 260 °C
6.40 µin/in-°F

@Temperature 70.0 - 500 °F
11.8 µm/m-°C

@Temperature 21.1 - 427 °C
6.58 µin/in-°F

@Temperature 70.0 - 800 °F
12.1 µm/m-°C

@Temperature 21.1 - 538 °C
6.72 µin/in-°F

@Temperature 70.0 - 1000 °F
Component Elements Properties Metric English Comments
Carbon, C 0.85 %
0.85 %
Chromium, Cr 4.15 %
4.15 %
Iron, Fe >= 81 %
>= 81 %
as balance
Manganese, Mn 0.30 %
0.30 %
Molybdenum, Mo 5.0 %
5.0 %
Silicon, Si 0.30 %
0.30 %
Sulfur, S <= 0.030 %
<= 0.030 %
Tungsten, W 6.4 %
6.4 %
Vanadium, V 1.95 %
1.95 %
Chemical Properties Metric English Comments
Critical Temperature 832 °C
1530 °F