Borealis FG5199 Linear Low Density Polyethylene

Category Polymer , Thermoplastic , Polyethylene (PE) , LLDPE , Linear Low Density Polyethylene (LLDPE), Film Grade
Manufacturer Borealis
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Borealis FG5199 Linear Low Density Polyethylene.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
FG5199 is a Butene Linear Low Density Polyethylene for Film Extrusion. Includes antioxidant, anti-Fog and cling additives. The grade is developed for blown cling film. Film made from FG5199 is suitable for manual wrapping of various foodstuffs e.g. cheese, meat and vegetables. Applications: cling, food packaging, food wrap film, and lamination films.Information provided by Borealis AG
Physical Properties Metric English Comments
Density 0.919 g/cc
0.0332 lb/in³
ISO 1183
Melt Flow 1.25 g/10 min

@Load 2.16 kg,
Temperature 190 °C
1.25 g/10 min

@Load 4.76 lb,
Temperature 374 °F
ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength, Yield 11.0 MPa
1600 psi
TD; ISO 527-3
Film Elongation at Break, MD 550 %
550 %
ISO 527-3
Film Elongation at Break, TD 710 %
710 %
ISO 527-3
Elmendorf Tear Strength, MD 2.04 g/micron
51.8 g/mil
ISO 6383/2
Elmendorf Tear Strength, TD 15.49 g/micron
393.4 g/mil
ISO 6383/2
Dart Drop Test 70.0 g

@Thickness 0.0250 mm
0.154 lb

@Thickness 0.000984 in
ISO 7765-1
Film Tensile Strength at Break, MD 32.0 MPa
4640 psi
ISO 527-3
Film Tensile Strength at Break, TD 28.0 MPa
4060 psi
ISO 527-3
Thermal Properties Metric English Comments
Melting Point 121 °C
250 °F
ISO 11357-3