Properties: The iCARe™ Save product family comes with guaranteed losses at 400Hz and indicative maximum values at 700Hz. These values are representative of the steel’s behaviour at high frequencies.Advantages: Save grades enable you to reduce the iron losses from the stators of synchronous machines. They are particularly useful for reducing iron losses in high-speed hybrid and electric traction machines, and generators which extend the range of electric vehicles.Applications: Save grades are most effective at reducing iron losses from machine parts which are subject to high base frequencies and additional harmonics. Save thus helps to improve machine efficiency, which leads to an increase in power density. Power density can be tuned to create a lighter, smaller machine, or a more powerful machine for a given weight. Driving range is extended as Save reduces machine weight and costs and saves battery energy.Recommendations for use: Save grades can be used immediately after lamination punching. The punching effect can be eliminated by performing a stress relief annealing. This optimises their performance in applications with fine teeth, and enables a substantial part of the lower frequency area to be exploited. A C5-type coating is recommended. Save stacks can be produced using existing assembly techniques such as interlocking or welding.Information provided by ArcelorMittal
Physical Properties Metric English Comments
Density 7.60 g/cc
0.275 lb/in³
Mechanical Properties Metric English Comments
Hardness, Vickers 200 - 230
200 - 230
L direction
200 - 230
200 - 230
T direction
Tensile Strength, Ultimate 520 - 560 MPa
75400 - 81200 psi
L direction
535 - 575 MPa
77600 - 83400 psi
T direction
Tensile Strength, Yield 410 - 450 MPa
59500 - 65300 psi
L direction
425 - 465 MPa
61600 - 67400 psi
T direction
Elongation at Break 12 - 25 %
12 - 25 %
L direction
12 - 25 %
12 - 25 %
T direction
Magnetic Properties Metric English Comments
Core Loss <= 15.0 W/kg

@Frequency 400 Hz
<= 6.80 W/lb

@Frequency 400 Hz
at 1T, Guaranteed
<= 37.0 W/kg

@Frequency 700 Hz
<= 16.8 W/lb

@Frequency 700 Hz
at 1T, Indicative
Descriptive Properties Value Comments
Anisotropy >15%
400 Hz at 1T
Polarization >1.49 T
at 2,500 A/m
>1.6 T
at 5,000 A/m
>1.7 T
at 10,000 A/m