Touchstone CFOAM® 20 Structural Carbon Foam

Category Carbon , Other Engineering Material , Composite Core Material
Manufacturer Touchstone Research Laboratory
Trade Name CFOAM®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Touchstone CFOAM® 20 Structural Carbon Foam.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
CFOAM, developed by Touchstone Research Laboratory, Ltd., is a next generation structural material which is inexpensive, lightweight, fire-resistant, impact-absorbing, and which can be thermally insulating or conducting and whose electrical conductivity can be varied over seven orders of magnitude. It can be fabricated in a variety of shapes, sizes, and densities to meet the property requirements of specific applications.These foams will not off-gas at elevated temperatures and will not support ignition. Unlike most metals and ceramics, CFOAM mechanical properties do not deteriorate with increased temperature if protected from oxidization, making carbon foams an attractive thermal protection material. Carbon foams also are tolerant to impact damage and can be repaired in-place using carbonaceous adhesives. They can be bonded easily to dissimilar materials, such as metals or PMCs, for oxidation or further impact protection, respectively.Results from ASTM E1354, ASTM E1515, MIL-STD-1623, Coast Guard IMO, and FTP Code Part I and Part III indicate that CFOAM will pass all key fire tests including radiant panel, smoke generation, toxicity, cone calorimeter, fire resistance, and room corner tests.Information provided by Touchstone Research Laboratory.
Physical Properties Metric English Comments
Density 0.320 g/cc
0.0116 lb/in³
ASTM D1622
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate >= 2.07 MPa
>= 300 psi
ASTM C297
Tensile Modulus 0.414 GPa
60.0 ksi
ASTM C297
Compressive Strength >= 7.58 MPa
>= 1100 psi
ASTM D365
Compressive Modulus 0.621 GPa
90.0 ksi
ASTM D365
Shear Strength >= 1.31 MPa
>= 190 psi
Torsional Shear
Thermal Properties Metric English Comments
CTE, linear 5.04 µm/m-°C
2.80 µin/in-°F
Thermal Conductivity 0.250 W/m-K

@Temperature 23.0 °C
1.74 BTU-in/hr-ft²-°F

@Temperature 73.4 °F
0.700 W/m-K

@Temperature 500 °C
4.86 BTU-in/hr-ft²-°F

@Temperature 932 °F
1.00 W/m-K

@Temperature 1000 °C
6.94 BTU-in/hr-ft²-°F

@Temperature 1830 °F
4.00 W/m-K

@Temperature 2000 °C
27.8 BTU-in/hr-ft²-°F

@Temperature 3630 °F
Maximum Service Temperature, Air >= 299 °C
>= 570 °F
Maximum Service Temperature, Inert >= 3000 °C
>= 5430 °F
Electrical Properties Metric English Comments
Electrical Resistivity 0.069 ohm-cm
0.069 ohm-cm
Standard
0.0025 - 2.5e+6 ohm-cm
0.0025 - 2.5e+6 ohm-cm
Tailorable; ASTM D4496
Descriptive Properties Value Comments
Fire Resistance ISO 1182, ASTM E1354, ASTM E119, IMO FTP Cote Pt. I & III, UL1709
Pass