Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay Specialty Polymers Cogegum® AFR/720 Polyolefin, Unspecified  (discontinued **)

Category Polymer , Thermoplastic , Polyolefin
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Solvay Specialty Polymers Cogegum® AFR/720 Polyolefin, Unspecified  (discontinued **).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Cogegum® HFFR -Halogen Free Fire Retardant compound Polyolefin based thermoplastic compound containing a fire retardant system that contributes to give the cable self-extinguish properties without halogenidric acids evolution; furthermore, toxic and corrosive gases emission and smoke generation are particularly reduced. These characteristics make this compound suitable in all applications where the fire behavior of cable materials is one of the main concerns to be considered in establishing a high safety level in public places. This material complies with RoHS requirements. standard complying - EN 50363-0 M1, M9; EN 50363-7 TI6, TI7; IEC 60502-1 ST8; Cenelec HD 624.7 S1; Cenelec HD 624.6 S1; VDE 0207 HM2, HM5, HJ2; IEC 60092 SHF1; UNE 211002 TIZ1; UNE 21123-4Additional Information: Tests reported are performed on pressed or extruded specimens Coloring - EVA or PE based masterbatches added at 1.2-1.5% by weight; in order to avoid scotching problems during processing, predrying of colour masterbatch is suggested if moisture absorption occurred during storage (4-6 hours at 50-60°C). Storage - The product must be stored under the following conditions: -- closed and undamaged bags -- ambient temperature not exceeding 35°C -- avoid direct exposure to sunlight and weathering - Product alterations could occur due to extended period of storage - Shelf life: 12 months - Solvay Specialty Polymers accepts no liability of any kind in case the above mentioned conditions are not fulfilled. Packaging - 25 kg moisture-resistant bags on 1375 kg pallet - 1000 kg carton boxExtrusion Notes: Extrusion equipment - standard extruders for thermoplastics equipped with low compression screw (1:1.2-1.4 compression ratio and 20-25 L/D ratio are suggested), and an adequate barrel thermoregulation - don't use screw thermoregulation - filter net: not necessary; in case, use 40-80 mesh/cm² max. Anyway the use of the breaker plate is advisable, in particular using low compression screwsInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Specific Gravity 1.48 g/cc
1.48 g/cc
ASTM D792
ESCR 10% Igepal® 1000 hour
<br>@Thickness 3.00 mm,<br> Temperature 50.0 °C
1000 hour
<br>@Thickness 0.118 in,<br> Temperature 122 °F
Condition A, Compression Molded; ASTM D1693
Melt Flow 3.9 g/10 min
<br>@Load 21.6 kg,<br> Temperature 150 °C
3.9 g/10 min
<br>@Load 47.6 lb,<br> Temperature 302 °F
Internal Method
Mechanical Properties Metric English Comments
Hardness, Shore D 47
47
ISO 868
Tensile Strength at Break 15.2 MPa
2200 psi
IEC 60811
Elongation at Break 190 %
190 %
IEC 60811
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 280 °C
536 °F
Temperature Index (Burning); NES 715
Oxygen Index 39 %
39 %
ASTM D2863
Electrical Properties Metric English Comments
Volume Resistivity 5.50e+12 ohm-cm
<br>@Temperature 70.0 °C
5.50e+12 ohm-cm
<br>@Temperature 158 °F
IEC 60502
4.10e+14 ohm-cm
<br>@Temperature 20.0 °C
4.10e+14 ohm-cm
<br>@Temperature 68.0 °F
IEC 60502
Insulation Resistivity 20.0 Megaohm/1000 m
<br>@Temperature 70.0 °C
65.6 Megaohm/1000 ft
<br>@Temperature 158 °F
IEC 60502
1500 Megaohm/1000 m
<br>@Temperature 20.0 °C
4920 Megaohm/1000 ft
<br>@Temperature 68.0 °F
IEC 60502
Processing Properties Metric English Comments
Processing Temperature 150 - 170 °C
302 - 338 °F
Collar Temperature
Zone 1 130 - 150 °C
266 - 302 °F
Zone 2 130 - 160 °C
266 - 320 °F
Zone 3 140 - 160 °C
284 - 320 °F
Zone 4 140 - 160 °C
284 - 320 °F
Die Temperature 150 - 180 °C
302 - 356 °F
Head Temperature 150 - 170 °C
302 - 338 °F
Descriptive Properties Value Comments
Availability Asia Pacific
Europe
North America
Bending Test Pass
-25°C; IEC 60811
Calorific Potential 16.2 MJ/kg
ISO 1716; Upper (gross)
Cold Impact Pass
IEC 60811; -25°C
Corrosive Gas in Smoke < 10.0 µS/mm
Conductivity IEC 60754-2
pH > 4.30
Features Flame Retardant
Halogen Free
Low Smoke Emission
Low Toxicity
Self Extinguishing
Generic Polyolefin, Unspecified
Halogenidric Acid Emissions < 0.10%
Heat Shock Pass
IEC 60811; 150°C
Hot Pressure Test < 50%
90°C; max penetration, K=0.6; IEC 60811
Hydrocarbons Immersion Test, 25°C, 4 hr -12
CEI 20-34/0-1; % Change in Tensile Strength
-5
CEI 20-34/0-1; % Change in Tensile Elongation
Mechanical Properties After Aging in Air Oven, 100°C, 168 hr -10
IEC 60811, %Change in Tensile Elongation
4
IEC 60811, %Change in Tensile Strength
Mechanical Properties After Aging in Air Oven, 80°C, 168 hr -12
IEC 60811, %Change in Tensile Elongation
-5
IEC 60811, %Change in Tensile Strength
RoHS Compliance RoHS Compliant
SAE 20 Oil Immersion Test, 70°C, 4 hr -24
% Change in Tensile Strength
4
% Change in Tensile Elongation
Uses Cable Jacketing
Low Voltage Insulation
Wire & Cable Applications
Water Absorption (mg/cm²) 3.5
100°C; 24 hr; IEC 60811