Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Schott CONTURAX® Borosilicate Glass

Category Ceramic , Glass
Manufacturer Schott North America
Trade Name
Port Shanghai port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Schott CONTURAX® Borosilicate Glass.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Borosilicate glass tubing and rod, varying types of inner and outer shapes Lighting, giftware, and decoration The heavy metal content for the elements lead, cadmium, mercury, and hexavalent chromium is below 100 ppmInformation provided by SCHOTT AG.
Physical Properties Metric English Comments
Density 2.23 g/cc
<br>@Temperature 25.0 °C
0.0806 lb/in³
<br>@Temperature 77.0 °F
Mechanical Properties Metric English Comments
Modulus of Elasticity 63.0 GPa
9140 ksi
Poissons Ratio 0.20
0.20
Shear Modulus 26.3 GPa
3810 ksi
Calculated
Thermal Properties Metric English Comments
CTE, linear 3.30 µm/m-°C
<br>@Temperature 20.0 - 300 °C
1.83 µin/in-°F
<br>@Temperature 68.0 - 572 °F
ISO 7991
Thermal Conductivity 1.20 W/m-K
<br>@Temperature 90.0 °C
8.33 BTU-in/hr-ft²-°F
<br>@Temperature 194 °F
Transformation Temperature, Tg 525 °C
977 °F
ISO 7884-8
Softening Point 825 °C
1520 °F
Viscosity 10&lt;sup&gt;7.6&lt;/sup&gt; dPa s; ISO 7884-3
Working Point 1260 °C
2300 °F
Viscosity 10&lt;sup&gt;4&lt;/sup&gt; dPa s; ISO 7884-2
Annealing Point 560 °C
1040 °F
Viscosity 10&lt;sup&gt;13&lt;/sup&gt; dPa s; ISO 7884-4
Optical Properties Metric English Comments
Refractive Index 1.473
<br>@Wavelength 587.6 nm
1.473
<br>@Wavelength 587.6 nm
Electrical Properties Metric English Comments
Volume Resistivity 3.20e+6 ohm-cm
<br>@Temperature 350 °C
3.20e+6 ohm-cm
<br>@Temperature 662 °F
1.00e+8 ohm-cm
<br>@Temperature 250 °C
1.00e+8 ohm-cm
<br>@Temperature 482 °F
Dielectric Constant 4.6
<br>@Frequency 1.00e+6 Hz,<br> Temperature 25.0 °C
4.6
<br>@Frequency 1.00e+6 Hz,<br> Temperature 77.0 °F
Dielectric Loss Index 0.0037
<br>@Frequency 1.00e+6 Hz,<br> Temperature 25.0 °C
0.0037
<br>@Frequency 1.00e+6 Hz,<br> Temperature 77.0 °F
Chemical Properties Metric English Comments
Acid Class, SR 1
1
DIN 12116
Alkali Class, AR 2
2
ISO 695
Descriptive Properties Value Comments
Hydrolytic Resistance Class HGB 1
ISO 719
Stress-optical Coefficient K (10-6mm2N-1) 4
DIN 52314
tk100(°C) 250