| Category | Polymer , Thermoplastic , Polyphenylene Sulfide (PPS) |
| Manufacturer | SABIC Innovative Plastics (GE Plastics) |
| Trade Name | LNP STAT-KON |
| Port | Shanghai port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | SABIC Innovative Plastics LNP STAT-KON OE006A PPS - Branched.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.44 g/cc | 0.0520 lb/in³ | ASTM D792 |
| 1.44 g/cc | 0.0520 lb/in³ | ISO 1183 | |
| Moisture Absorption | 0.0200 % | 0.0200 % | 50% RH, 24 hrs; ASTM D570 |
| 0.0300 % | 0.0300 % | 23°C / 50% RH; ISO 62 | |
| Linear Mold Shrinkage, Flow | 0.00080 cm/cm @Time 86400 sec |
0.00080 in/in @Time 24.0 hour |
ISO 294 |
| 0.0010 cm/cm @Time 86400 sec |
0.0010 in/in @Time 24.0 hour |
ASTM D955 | |
| Linear Mold Shrinkage, Transverse | 0.0040 cm/cm @Time 86400 sec |
0.0040 in/in @Time 24.0 hour |
ASTM D955 |
| 0.0040 cm/cm @Time 86400 sec |
0.0040 in/in @Time 24.0 hour |
ISO 294 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 204 MPa | 29600 psi | ISO 527 |
| 210 MPa | 30500 psi | ASTM D638 | |
| Elongation at Break | 1.0 % | 1.0 % | ISO 527 |
| 1.1 % | 1.1 % | ASTM D638 | |
| Tensile Modulus | 25.45 GPa | 3691 ksi | 1 mm/min; ISO 527 |
| 32.75 GPa | 4750 ksi | 50 mm/min; ASTM D638 | |
| Flexural Strength | 304 MPa | 44100 psi | ASTM D790 |
| 311 MPa | 45100 psi | ISO 178 | |
| Flexural Modulus | 23.51 GPa | 3410 ksi | ASTM D790 |
| 24.72 GPa | 3585 ksi | ISO 178 | |
| Izod Impact, Notched | 0.490 J/cm | 0.918 ft-lb/in | ASTM D256 |
| Izod Impact, Unnotched | 4.37 J/cm | 8.19 ft-lb/in | ASTM D4812 |
| Izod Impact, Notched (ISO) | 5.00 kJ/m² | 2.38 ft-lb/in² | 80*10*4; ISO 180/1A |
| Izod Impact, Unnotched (ISO) | 28.0 kJ/m² | 13.3 ft-lb/in² | 80*10*4; ISO 180/1U |
| Dart Drop, Total Energy | 3.00 J | 2.21 ft-lb | Instrumented Impact Energy @ peak; ASTM D3763 |
| Impact Test | 1.00 J | 0.738 ft-lb | Multiaxial Impact; ISO 6603 |
| Coefficient of Friction, Dynamic | 1.6 | 1.6 | ASTM D3702 Modified |
| Coefficient of Friction, Static | 1.38 | 1.38 | ASTM D3702 Modified |
| K (wear) Factor | 1730 x 10-8 mm³/N-M | 857 x 10-10 in³-min/ft-lb-hr | Washer; ASTM D3702 Modified |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 7.20 µm/m-°C @Temperature -40.0 - 40.0 °C |
4.00 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 8.70 µm/m-°C @Temperature -40.0 - 40.0 °C |
4.83 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| CTE, linear, Transverse to Flow | 39.6 µm/m-°C @Temperature -40.0 - 40.0 °C |
22.0 µin/in-°F @Temperature -40.0 - 104 °F |
ASTM E 831 |
| 40.8 µm/m-°C @Temperature -40.0 - 40.0 °C |
22.7 µin/in-°F @Temperature -40.0 - 104 °F |
ISO 11359-2 | |
| Flammability, UL94 | V-0 @Thickness 1.00 mm |
V-0 @Thickness 0.0394 in |
UL 94 by SABIC-IP |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Surface Resistance | 100 - 1.00e+6 ohm | 100 - 1.00e+6 ohm | ASTM D257 |