Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Quadrant EPP Fluorosint® 207 PTFE + mica, compression moulded (ISO Data)

Category Polymer , Thermoplastic , Fluoropolymer , PTFE , Polytetrafluoroethylene (PTFE), Mica Filled
Manufacturer Quadrant Engineering Plastics Products
Trade Name Fluorosint®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Quadrant EPP Fluorosint® 207 PTFE + mica, compression moulded (ISO Data).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
This material has a food contact compliant composition which, in combination with the good mechanical performance, dimensional stability, sliding and wear properties and inherent outstanding chemical and hydrolysis resistance of Fluorosint, opens numerous application possibilities in food, pharmaceutical and chemical processing industries High maximum allowable service temperature in air (260°C continuously) Excellent chemical and hydrolysis resistance Outstanding UV- and weather resistance Physiologically inert (suitable for food contact, except Fluorosint 500, Fluorosint MT-01) Inherent low flammability Good electrical insulating properties
Physical Properties Metric English Comments
Density 2.30 g/cc
0.0831 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium <= 0.10 %
<= 0.10 %
50% RH
Water Absorption at Saturation 1.0 - 2.0 %
1.0 - 2.0 %
Mechanical Properties Metric English Comments
Hardness, Rockwell R 50
50
ISO 2039-2
Hardness, Shore D 60
60
Ball Indentation Hardness 40.0 MPa
5800 psi
ISO 2039-1
Tensile Strength 10.0 MPa
1450 psi
at Yield; ISO 527-1/-2
Elongation at Break >= 50 %
>= 50 %
ISO 527-1/-2
Elongation at Yield 4.0 %
4.0 %
ISO 527-1/-2
Tensile Modulus 1.45 GPa
210 ksi
ISO 527-1/-2
Flexural Strength 14.0 MPa
2030 psi
Compressive Strength 10.5 MPa

@Strain 1 %
1520 psi

@Strain 1 %
ISO 604
15.0 MPa

@Strain 2 %
2180 psi

@Strain 2 %
ISO 604
20.0 MPa

@Strain 5 %
2900 psi

@Strain 5 %
ISO 604
K Factor (ISO) 5.0 µm/km
5.0 µm/km
Charpy Impact Unnotched 3.00 J/cm²
14.3 ft-lb/in²
ISO 179-1/1eU
Charpy Impact, Notched 0.750 J/cm²
3.57 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.15 - 0.25
0.15 - 0.25
Limiting Pressure Velocity 0.250 MPa-m/sec
7140 psi-ft/min
at 1 m/s unlubricated
0.400 MPa-m/sec
11400 psi-ft/min
at 0.1 m/s unlubricated
Thermal Properties Metric English Comments
CTE, linear 85.0 µm/m-°C

@Temperature 23.0 - 100 °C
47.2 µin/in-°F

@Temperature 73.4 - 212 °F
Melting Point 327 °C
621 °F
DSC, 10°C/min.; ISO 11357-1/-3
Maximum Service Temperature, Air 260 °C
500 °F
Continuous
Deflection Temperature at 1.8 MPa (264 psi) 100 °C
212 °F
ISO 75-1/-2
Flammability, UL94 V-0
V-0
Oxygen Index >= 95 %
>= 95 %
ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity >= 1.0e+13 ohm-cm
>= 1.0e+13 ohm-cm
IEC 60093
Surface Resistivity per Square >= 1.0e+13 ohm
>= 1.0e+13 ohm
IEC 60093
Dielectric Strength 8.00 kV/mm
203 kV/in
Compliance Properties Metric English Comments
3A-Dairy No
No
European Food 1935/2004 No
No
FDA Yes
Yes
USP Class VI No
No
Chemical Resistance Properties Metric English Comments
Acids, Strong (pH 1-3) Acceptable
Acceptable
Acids, Weak Acceptable
Acceptable
Alcohols Acceptable
Acceptable
Alkalies, Strong (pH 11-14) Unacceptable
Unacceptable
Alkalies, Weak Acceptable
Acceptable
Chlorinated Solvents Acceptable
Acceptable
Continuous Sunlight Acceptable
Acceptable
Hot Water / Steam Limited
Limited
Hydrocarbons - Aliphatic Acceptable
Acceptable
Hydrocarbons - Aromatic Acceptable
Acceptable
Inorganic Salt Solutions Acceptable
Acceptable
Ketones, Esters Acceptable
Acceptable