Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

DuPont Teijin Films Mylar® MDA Polyester Film, 300 Gauge

Category Polymer , Film , Thermoplastic , Polyester, TP , Polyester Film
Manufacturer DuPont Teijin Films (DTF)
Trade Name Mylar®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF DuPont Teijin Films Mylar® MDA Polyester Film, 300 Gauge.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Mylar® MDA films are tough, general purpose films that are transparent in 48 through 92 gauge and translucent in heavier gauges. They have a rough surface to provide ease of handling, good adhesion, and processability. They are used for a broad range of industrial applications and may be suitable for use in medical applications.General Product Info: Mylar® MDA films have balanced tensile properties and excellent resistance to moisture and most chemicals. They can withstand temperature extremes from -100°F to 300ºF. Mylar® does not become brittle with age under normal conditions, because it contains no plasticizers. Typical Applications:Apparel staysBook jacketsCarbon ribbonControl TapeDrumheadsDuct LinersIdentificationsMedical ApplicationsMembrane touch switchesMetallized BasePressure Sensitive Labels (plain or metallized)Protective surfacingRelease linersRoll leaf (hot stamping)Spirit MastersApprovals: FDA Food Contact Status - All gauges of Mylar® MDA comply with the Food and Drug Administration regulation 21 CFR 177.1630 -- Polyethylene phthalate polymers. This regulation describes films which may be safely used in contact with all types of food excluding alcoholic beverages. Uncoated films such as Mylar® MDA can be used to contain foods during oven cooking or oven baking at temperatures above 250 °F.Information provided by DuPont.
Physical Properties Metric English Comments
Density 1.39 g/cc
0.0502 lb/in³
Typical Mylar®; ASTM D1505
Mechanical Properties Metric English Comments
Film Elongation at Break, MD 135 %
135 %
ASTM D882A
Film Elongation at Break, TD 110 %
110 %
ASTM D882A
Tensile Modulus 3.50 GPa
507 ksi
ASTM D882
Film Tensile Strength at Break, MD 186 MPa
27000 psi
ASTM D882A
Film Tensile Strength at Break, TD 214 MPa
31000 psi
ASTM D882A
Thermal Properties Metric English Comments
Specific Heat Capacity 1.17 J/g-°C
0.280 BTU/lb-°F
Typical Mylar®
Melting Point 254 °C
489 °F
Typical Mylar® via DSC
Maximum Service Temperature, Air 149 °C
300 °F
Maximum Service Temperature, Inert -73.3 °C
-100 °F
Shrinkage, MD 1.2 %

@Temperature 150 °C,
Time 1800 sec
1.2 %

@Temperature 302 °F,
Time 0.500 hour
Unrestrained
Shrinkage, TD 0.80 %

@Temperature 150 °C,
Time 1800 sec
0.80 %

@Temperature 302 °F,
Time 0.500 hour
Unrestrained
Optical Properties Metric English Comments
Refractive Index 1.64 - 1.67
1.64 - 1.67
typical of Mylar®
Haze 14 - 50 %
14 - 50 %
ASTM D1003
Descriptive Properties Value Comments
Yield (nominal) 6600 in2/lb
Users viewing this material also viewed the following: