| Category | Polymer , Thermoplastic , Polyphthalamide (PPA) , Polyphthalamide (PPA), 40% Glass Fiber Reinforced |
| Manufacturer | DuPont Performance Polymers |
| Trade Name | Zytel® HTN |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | DuPont Performance Polymers Zytel® HTN 54G35EF BK420 Polyphthalamide (PPA)
(Unverified Data**).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.42 g/cc | 0.0513 lb/in³ | DAM; ISO 1183 |
| Linear Mold Shrinkage, Flow | 0.0020 cm/cm | 0.0020 in/in | DAM; ISO 294-4 2577 |
| Linear Mold Shrinkage, Transverse | 0.0050 cm/cm | 0.0050 in/in | DAM; ISO 294-4 2577 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 185 MPa | 26800 psi | DAM; ISO 527-1/-2 |
| Tensile Stress | 1.39 MPa @Strain 0.0300 %, Temperature -20.0 °C |
202 psi @Strain 0.0300 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 |
| 1.71 MPa @Strain 0.0600 %, Temperature 23.0 °C |
248 psi @Strain 0.0600 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 1.83 MPa @Strain 0.0200 %, Temperature 0.000 °C |
265 psi @Strain 0.0200 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 2.30 MPa @Strain 0.0500 %, Temperature 0.000 °C |
334 psi @Strain 0.0500 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 2.52 MPa @Strain 0.0600 %, Temperature -20.0 °C |
365 psi @Strain 0.0600 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 3.23 MPa @Strain 0.0800 %, Temperature 150 °C |
468 psi @Strain 0.0800 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 3.25 MPa @Strain 0.0700 %, Temperature 180 °C |
471 psi @Strain 0.0700 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 3.35 MPa @Strain 0.0700 %, Temperature 150 °C |
486 psi @Strain 0.0700 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 4.01 MPa @Strain 0.0700 %, Temperature 90.0 °C |
582 psi @Strain 0.0700 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 4.49 MPa @Strain 0.0300 %, Temperature 90.0 °C |
651 psi @Strain 0.0300 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 4.99 MPa @Strain 0.0600 %, Temperature 40.0 °C |
724 psi @Strain 0.0600 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 5.23 MPa @Strain 0.0500 %, Temperature 40.0 °C |
759 psi @Strain 0.0500 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 5.29 MPa @Strain 0.0500 %, Temperature 23.0 °C |
767 psi @Strain 0.0500 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 10.69 MPa @Strain 0.120 %, Temperature 0.000 °C |
1550 psi @Strain 0.120 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 11.68 MPa @Strain 0.330 %, Temperature 180 °C |
1694 psi @Strain 0.330 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 11.76 MPa @Strain 0.240 %, Temperature 90.0 °C |
1706 psi @Strain 0.240 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 11.8 MPa @Strain 0.290 %, Temperature 150 °C |
1710 psi @Strain 0.290 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 12.54 MPa @Strain 0.130 %, Temperature -20.0 °C |
1819 psi @Strain 0.130 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 13.02 MPa @Strain 0.170 %, Temperature 23.0 °C |
1888 psi @Strain 0.170 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 13.84 MPa @Strain 0.410 %, Temperature 150 °C |
2007 psi @Strain 0.410 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 14.11 MPa @Strain 0.130 %, Temperature 90.0 °C |
2046 psi @Strain 0.130 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 14.97 MPa @Strain 0.170 %, Temperature 40.0 °C |
2171 psi @Strain 0.170 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 15.73 MPa @Strain 0.160 %, Temperature 40.0 °C |
2281 psi @Strain 0.160 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 15.77 MPa @Strain 0.170 %, Temperature 0.000 °C |
2287 psi @Strain 0.170 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 16.41 MPa @Strain 0.170 %, Temperature 23.0 °C |
2380 psi @Strain 0.170 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 17.13 MPa @Strain 0.200 %, Temperature -20.0 °C |
2485 psi @Strain 0.200 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 23.17 MPa @Strain 0.240 %, Temperature 90.0 °C |
3361 psi @Strain 0.240 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 23.18 MPa @Strain 0.240 %, Temperature 0.000 °C |
3362 psi @Strain 0.240 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 27.22 MPa @Strain 0.270 %, Temperature 40.0 °C |
3948 psi @Strain 0.270 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 30.8 MPa @Strain 1.47 %, Temperature 180 °C |
4470 psi @Strain 1.47 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 32.17 MPa @Strain 0.320 %, Temperature -20.0 °C |
4666 psi @Strain 0.320 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 32.53 MPa @Strain 1.57 %, Temperature 150 °C |
4718 psi @Strain 1.57 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 33.5 MPa @Strain 0.360 %, Temperature 40.0 °C |
4860 psi @Strain 0.360 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 34.98 MPa @Strain 0.380 %, Temperature 23.0 °C |
5073 psi @Strain 0.380 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 36.08 MPa @Strain 1.37 %, Temperature 150 °C |
5233 psi @Strain 1.37 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 36.26 MPa @Strain 0.360 %, Temperature 23.0 °C |
5259 psi @Strain 0.360 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 38.61 MPa @Strain 1.11 %, Temperature 90.0 °C |
5600 psi @Strain 1.11 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 39.92 MPa @Strain 2.76 %, Temperature 180 °C |
5790 psi @Strain 2.76 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 41.83 MPa @Strain 2.87 %, Temperature 150 °C |
6067 psi @Strain 2.87 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 46.42 MPa @Strain 0.470 %, Temperature 0.000 °C |
6733 psi @Strain 0.470 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 47.69 MPa @Strain 2.56 %, Temperature 150 °C |
6917 psi @Strain 2.56 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 52.15 MPa @Strain 7.00 %, Temperature 180 °C |
7564 psi @Strain 7.00 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 52.83 MPa @Strain 2.15 %, Temperature 90.0 °C |
7662 psi @Strain 2.15 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 53.14 MPa @Strain 7.01 %, Temperature 150 °C |
7707 psi @Strain 7.01 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 54.82 MPa @Strain 9.55 %, Temperature 180 °C |
7951 psi @Strain 9.55 %, Temperature 356 °F |
DAM; ISO 11403-1 -2 | |
| 54.94 MPa @Strain 9.70 %, Temperature 150 °C |
7968 psi @Strain 9.70 %, Temperature 302 °F |
50%RH; ISO 11403-1 -2 | |
| 57.46 MPa @Strain 0.600 %, Temperature -20.0 °C |
8334 psi @Strain 0.600 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 | |
| 59.82 MPa @Strain 0.690 %, Temperature 90.0 °C |
8676 psi @Strain 0.690 %, Temperature 194 °F |
DAM; ISO 11403-1 -2 | |
| 62.9 MPa @Strain 6.42 %, Temperature 150 °C |
9120 psi @Strain 6.42 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 65.23 MPa @Strain 0.720 %, Temperature 40.0 °C |
9461 psi @Strain 0.720 %, Temperature 104 °F |
50%RH; ISO 11403-1 -2 | |
| 66.08 MPa @Strain 8.91 %, Temperature 150 °C |
9584 psi @Strain 8.91 %, Temperature 302 °F |
DAM; ISO 11403-1 -2 | |
| 68.14 MPa @Strain 5.88 %, Temperature 90.0 °C |
9883 psi @Strain 5.88 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 69.78 MPa @Strain 8.47 %, Temperature 90.0 °C |
10120 psi @Strain 8.47 %, Temperature 194 °F |
50%RH; ISO 11403-1 -2 | |
| 71.33 MPa @Strain 0.710 %, Temperature 0.000 °C |
10350 psi @Strain 0.710 %, Temperature 32.0 °F |
50%RH; ISO 11403-1 -2 | |
| 73.23 MPa @Strain 0.810 %, Temperature 40.0 °C |
10620 psi @Strain 0.810 %, Temperature 104 °F |
DAM; ISO 11403-1 -2 | |
| 77.37 MPa @Strain 0.830 %, Temperature 23.0 °C |
11220 psi @Strain 0.830 %, Temperature 73.4 °F |
50%RH; ISO 11403-1 -2 | |
| 80.94 MPa @Strain 0.750 %, Temperature -20.0 °C |
11740 psi @Strain 0.750 %, Temperature -4.00 °F |
50%RH; ISO 11403-1 -2 | |
| 81.51 MPa @Strain 0.860 %, Temperature 23.0 °C |
11820 psi @Strain 0.860 %, Temperature 73.4 °F |
DAM; ISO 11403-1 -2 | |
| 89.54 MPa @Strain 0.940 %, Temperature 0.000 °C |
12990 psi @Strain 0.940 %, Temperature 32.0 °F |
DAM; ISO 11403-1 -2 | |
| 101.41 MPa @Strain 1.07 %, Temperature -20.0 °C |
14708 psi @Strain 1.07 %, Temperature -4.00 °F |
DAM; ISO 11403-1 -2 |