| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.34 g/cc | 0.0484 lb/in³ | DAM; ISO 1183 |
| Linear Mold Shrinkage, Flow | 0.0010 cm/cm @Thickness 2.00 mm |
0.0010 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Linear Mold Shrinkage, Transverse | 0.0060 cm/cm @Thickness 2.00 mm |
0.0060 in/in @Thickness 0.0787 in |
DAM; ISO 294-4 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 53 | 53 | 50%RH; ISO 2039/2 |
| 81 | 81 | DAM; ISO 2039/2 | |
| Hardness, Rockwell R | 113 | 113 | 50%RH; ISO 2039/2 |
| 116 | 116 | DAM; ISO 2039/2 | |
| Tensile Strength at Break | 60.0 MPa @Temperature 150 °C |
8700 psi @Temperature 302 °F |
50%RH; ISO 527 |
| 66.0 MPa @Temperature 120 °C |
9570 psi @Temperature 248 °F |
50%RH; ISO 527 | |
| 67.0 MPa @Temperature 150 °C |
9720 psi @Temperature 302 °F |
DAM; ISO 527 | |
| 71.0 MPa @Temperature 100 °C |
10300 psi @Temperature 212 °F |
50%RH; ISO 527 | |
| 75.0 MPa @Temperature 120 °C |
10900 psi @Temperature 248 °F |
DAM; ISO 527 | |
| 77.0 MPa @Temperature 80.0 °C |
11200 psi @Temperature 176 °F |
50%RH; ISO 527 | |
| 82.0 MPa @Temperature 100 °C |
11900 psi @Temperature 212 °F |
DAM; ISO 527 | |
| 84.0 MPa @Temperature 60.0 °C |
12200 psi @Temperature 140 °F |
50%RH; ISO 527 | |
| 90.0 MPa @Temperature 80.0 °C |
13100 psi @Temperature 176 °F |
DAM; ISO 527 | |
| 102 MPa @Temperature 60.0 °C |
14800 psi @Temperature 140 °F |
DAM; ISO 527 | |
| 115 MPa @Temperature 23.0 °C |
16700 psi @Temperature 73.4 °F |
50%RH; ISO 527 | |
| 144 MPa @Temperature 0.000 °C |
20900 psi @Temperature 32.0 °F |
50%RH; ISO 527 | |
| 150 MPa @Temperature 23.0 °C |
21800 psi @Temperature 73.4 °F |
DAM; ISO 527 | |
| 167 MPa @Temperature 0.000 °C |
24200 psi @Temperature 32.0 °F |
DAM; ISO 527 | |
| 205 MPa @Temperature -40.0 °C |
29700 psi @Temperature -40.0 °F |
50%RH; ISO 527 | |
| 220 MPa @Temperature -40.0 °C |
31900 psi @Temperature -40.0 °F |
DAM; ISO 527 | |
| Elongation at Break | 4.0 % @Temperature 23.0 °C |
4.0 % @Temperature 73.4 °F |
DAM; ISO 527 |
| 5.4 % @Temperature -40.0 °C |
5.4 % @Temperature -40.0 °F |
50%RH; ISO 527 | |
| 5.5 % @Temperature 0.000 °C |
5.5 % @Temperature 32.0 °F |
DAM; ISO 527 | |
| 5.7 % @Temperature 0.000 °C |
5.7 % @Temperature 32.0 °F |
50%RH; ISO 527 | |
| 6.0 % @Temperature -40.0 °C |
6.0 % @Temperature -40.0 °F |
DAM; ISO 527 | |
| 8.5 % @Temperature 60.0 °C |
8.5 % @Temperature 140 °F |
DAM; ISO 527 | |
| 8.6 % @Temperature 23.0 °C |
8.6 % @Temperature 73.4 °F |
50%RH; ISO 527 | |
| 9.2 % @Temperature 60.0 °C |
9.2 % @Temperature 140 °F |
50%RH; ISO 527 | |
| 9.5 % @Temperature 80.0 °C |
9.5 % @Temperature 176 °F |
50%RH; ISO 527 | |
| 9.5 % @Temperature 100 °C |
9.5 % @Temperature 212 °F |
50%RH; ISO 527 | |
| 9.6 % @Temperature 80.0 °C |
9.6 % @Temperature 176 °F |
DAM; ISO 527 | |
| 10 % @Temperature 100 °C |
10 % @Temperature 212 °F |
DAM; ISO 527 | |
| 10.3 % @Temperature 120 °C |
10.3 % @Temperature 248 °F |
50%RH; ISO 527 | |
| 10.7 % @Temperature 120 °C |
10.7 % @Temperature 248 °F |
DAM; ISO 527 | |
| 11.2 % @Temperature 150 °C |
11.2 % @Temperature 302 °F |
50%RH; ISO 527 | |
| 11.6 % @Temperature 150 °C |
11.6 % @Temperature 302 °F |
DAM; ISO 527 | |
| Tensile Modulus | 3.746 GPa @Temperature 150 °C |
543.3 ksi @Temperature 302 °F |
50%RH; ISO 527 |
| 4.052 GPa @Temperature 150 °C |
587.7 ksi @Temperature 302 °F |
DAM; ISO 527 | |
| 4.223 GPa @Temperature 120 °C |
612.5 ksi @Temperature 248 °F |
50%RH; ISO 527 | |
| 4.384 GPa @Temperature 120 °C |
635.8 ksi @Temperature 248 °F |
DAM; ISO 527 | |
| 4.70 GPa @Temperature 100 °C |
682 ksi @Temperature 212 °F |
50%RH; ISO 527 | |
| 4.956 GPa @Temperature 100 °C |
718.8 ksi @Temperature 212 °F |
DAM; ISO 527 | |
| 5.182 GPa @Temperature 80.0 °C |
751.6 ksi @Temperature 176 °F |
50%RH; ISO 527 | |
| 5.518 GPa @Temperature 60.0 °C |
800.3 ksi @Temperature 140 °F |
50%RH; ISO 527 | |
| 5.614 GPa @Temperature 80.0 °C |
814.2 ksi @Temperature 176 °F |
DAM; ISO 527 | |
| 6.905 GPa @Temperature 60.0 °C |
1001 ksi @Temperature 140 °F |
DAM; ISO 527 | |
| 6.929 GPa @Temperature 23.0 °C |
1005 ksi @Temperature 73.4 °F |
50%RH; ISO 527 | |
| 9.00 GPa @Temperature 23.0 °C |
1310 ksi @Temperature 73.4 °F |
DAM; ISO 527 | |
| 9.074 GPa @Temperature 0.000 °C |
1316 ksi @Temperature 32.0 °F |
DAM; ISO 527 | |
| 9.286 GPa @Temperature 0.000 °C |
1347 ksi @Temperature 32.0 °F |
50%RH; ISO 527 | |
| 9.426 GPa @Temperature -40.0 °C |
1367 ksi @Temperature -40.0 °F |
DAM; ISO 527 | |
| 10.234 GPa @Temperature -40.0 °C |
1484.3 ksi @Temperature -40.0 °F |
50%RH; ISO 527 | |
| Flexural Modulus | 3.167 GPa @Temperature 150 °C |
459.3 ksi @Temperature 302 °F |
50%RH; ISO 178 |
| 3.33 GPa @Temperature 150 °C |
483 ksi @Temperature 302 °F |
DAM; ISO 178 | |
| 3.461 GPa @Temperature 120 °C |
502.0 ksi @Temperature 248 °F |
50%RH; ISO 178 | |
| 3.502 GPa @Temperature 120 °C |
507.9 ksi @Temperature 248 °F |
DAM; ISO 178 | |
| 3.633 GPa @Temperature 100 °C |
526.9 ksi @Temperature 212 °F |
50%RH; ISO 178 | |
| 3.651 GPa @Temperature 100 °C |
529.5 ksi @Temperature 212 °F |
DAM; ISO 178 | |
| 3.737 GPa @Temperature 80.0 °C |
542.0 ksi @Temperature 176 °F |
50%RH; ISO 178 | |
| 3.982 GPa @Temperature 80.0 °C |
577.5 ksi @Temperature 176 °F |
DAM; ISO 178 | |
| 4.006 GPa @Temperature 60.0 °C |
581.0 ksi @Temperature 140 °F |
50%RH; ISO 178 | |
| 4.461 GPa @Temperature 60.0 °C |
647.0 ksi @Temperature 140 °F |
DAM; ISO 178 | |
| 5.60 GPa @Temperature 23.0 °C |
812 ksi @Temperature 73.4 °F |
50%RH; ISO 178 | |
| 7.683 GPa @Temperature 23.0 °C |
1114 ksi @Temperature 73.4 °F |
DAM; ISO 178 | |
| 7.723 GPa @Temperature -40.0 °C |
1120 ksi @Temperature -40.0 °F |
DAM; ISO 178 | |
| 7.859 GPa @Temperature 0.000 °C |
1140 ksi @Temperature 32.0 °F |
DAM; ISO 178 | |
| 8.042 GPa @Temperature -40.0 °C |
1166 ksi @Temperature -40.0 °F |
50%RH; ISO 178 | |
| 8.082 GPa @Temperature 0.000 °C |
1172 ksi @Temperature 32.0 °F |
50%RH; ISO 178 | |
| Izod Impact, Notched (ISO) | 12.0 kJ/m² @Temperature -40.0 °C |
5.71 ft-lb/in² @Temperature -40.0 °F |
50%RH; ISO 180/1A |
| 15.0 kJ/m² @Temperature -40.0 °C |
7.14 ft-lb/in² @Temperature -40.0 °F |
DAM; ISO 180/1A | |
| 21.0 kJ/m² @Temperature 23.0 °C |
9.99 ft-lb/in² @Temperature 73.4 °F |
DAM; ISO 180/1A |