Carpenter 20Cb-3® Stainless Steel, Strip, Annealed at 1750°F (955°C) then Water Quenched

Category Metal , Ferrous Metal , Stainless Steel , T 300 Series Stainless Steel
Manufacturer Carpenter Technology Corporation (Cartech)
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Carpenter 20Cb-3® Stainless Steel, Strip, Annealed at 1750°F (955°C) then Water Quenched.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Data provided by Carpenter Technology Corporation.20Cb-3® is an austenitic stainless steel possessing excellent resistance to hot sulfuric acid and many other aggressive environments which would readily attack Type 316 stainless. This alloy exhibits superior resistance to stress-corrosion cracking in boiling 20 to 40% sulfuric acid. 20Cb-3 stainless is also stabilized to limit intergranular attack, even in the sensitized condition. Corrosion tests on annealed and sensitized material conducted in the Ferric Sulfate - 50% Sulfuric Acid Test resulted in rates of 0.002 inches per month maximum. Important advantages of 20Cb-3 stainless are its excellent mechanical properties and comparative ease of fabrication. The presence of columbium in the alloy minimizes the precipitation of carbides during welding. Assemblies usually have been placed in service in the as-welded condition.This material has found wide use in all phases of the chemical and allied industries. It has been used extensively in the processing of synthetic rubber, high-octane gasoline, solvents, explosives, plastics, synthetic fibers, heavy chemicals, organic chemicals, pharmaceuticals, and agrichemicals. 20Cb-3 stainless has also been used in SO2 scrubbers where acid content, such as sulfuric acid, is of more concern than high-halogen content, such as chlorides. Other applications have included use in fans, mixing tanks, agitators, distillation towers, heat exchangers, process piping, bubble caps, metal cleaning and pickling tanks, spray pickling equipment, pump shafts and rods, valve stems, bolts, nuts, washers, tie rods, continuous-line pickling equipment including racks, etc.20Cb-3® is a registered trademark of Carpenter Technology Corporation.
Physical Properties Metric English Comments
Density 8.08 g/cc
0.292 lb/in³
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 641 MPa
93000 psi
Tensile Strength, Yield 317 MPa

@Strain 0.200 %
46000 psi

@Strain 0.200 %
Elongation at Break 38 %
38 %
In 50 mm
Reduction of Area 62 %
62 %
Modulus of Elasticity 193 GPa
28000 ksi
In Tension
Poissons Ratio 0.31
0.31
Fatigue Strength 330 MPa

@# of Cycles 1.00e+7
47900 psi

@# of Cycles 1.00e+7
R.R. Moore Test, Smooth Rotating Beam
Shear Modulus 73.7 GPa
10700 ksi
Calculated
Thermal Properties Metric English Comments
CTE, linear 14.69 µm/m-°C

@Temperature 25.0 - 100 °C
8.161 µin/in-°F

@Temperature 77.0 - 212 °F
15.91 µm/m-°C

@Temperature 25.0 - 450 °C
8.839 µin/in-°F

@Temperature 77.0 - 842 °F
17.15 µm/m-°C

@Temperature 25.0 - 900 °C
9.528 µin/in-°F

@Temperature 77.0 - 1650 °F
Specific Heat Capacity 0.500 J/g-°C
0.120 BTU/lb-°F
Component Elements Properties Metric English Comments
Carbon, C <= 0.060 %
<= 0.060 %
Chromium, Cr 19 - 21 %
19 - 21 %
Copper, Cu 3.0 - 4.0 %
3.0 - 4.0 %
Iron, Fe 36 %
36 %
as remainder
Manganese, Mn <= 2.0 %
<= 2.0 %
Molybdenum, Mo 2.0 - 3.0 %
2.0 - 3.0 %
Nb + Ta <= 1.0 %
<= 1.0 %
Nickel, Ni 32.5 - 35 %
32.5 - 35 %
Niobium, Nb (Columbium, Cb) <= 1.0 %
<= 1.0 %
min Nb = 8 x C content
Phosphorous, P <= 0.035 %
<= 0.035 %
Silicon, Si <= 1.0 %
<= 1.0 %
Sulfur, S <= 0.035 %
<= 0.035 %
Tantalum, Ta <= 1.0 %
<= 1.0 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.0001082 ohm-cm
0.0001082 ohm-cm
Magnetic Permeability 1.002
1.002