Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

ATI Allegheny Ludlum Stainless Steel Type 201, Annealed (UNS S20100)

Category Metal , Ferrous Metal , Stainless Steel , T S20000 Series Stainless Steel
Manufacturer ATI Allegheny Ludlum
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF ATI Allegheny Ludlum Stainless Steel Type 201, Annealed (UNS S20100).pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Allegheny Ludlum Type 201 and 201L have the greatest tonnage of the Cr-Ni-Mn steels (200 series). Type 201 provides advantages over the 18-8 grades in certain applications. Lower cost manganese and nitrogen additions are partial substitutes for nickel making them more economical alloys. Because they possess a very desirable combination of economy plus good mechanical properties and corrosion resistance properties, they have been used in a wide variety of consumer and transportation applications.Balancing of alloying elements (austenitizers versus feritizer) in Type 201 produces an austenitic structure in the annealed condition even at subzero temperatures. This austenitic structure achieves significant strengthening through cold working of the material to produce the transformation to a stronger martensitic structure. Because of its high work hardening rate, it exhibits a high uniform elongation for improved stretchability for severe forming applications such as washing machine baskets.Typical applications for Types 201 and 201L are cookware bodies/lids, hose clamps, piston rings, transit car structural member, transit car roofing/siding, thermal window spacers, air bag containers, and truck trailer posts and door frames.Information provided by Allegheny Ludlum Corporation.
Physical Properties Metric English Comments
Density 7.86 g/cc
0.284 lb/in³
Mechanical Properties Metric English Comments
Hardness, Rockwell B 85

@Temperature 23.0 °C
85

@Temperature 73.4 °F
85

@Temperature 23.0 °C
85

@Temperature 73.4 °F
Tensile Strength, Ultimate 685 MPa

@Temperature 23.0 °C
99400 psi

@Temperature 73.4 °F
696 MPa

@Temperature 23.0 °C
101000 psi

@Temperature 73.4 °F
Tensile Strength, Yield 292 MPa

@Temperature 23.0 °C
42400 psi

@Temperature 73.4 °F
301 MPa

@Temperature 23.0 °C
43700 psi

@Temperature 73.4 °F
Elongation at Break 56 %

@Temperature 23.0 °C
56 %

@Temperature 73.4 °F
62.5 %

@Temperature 23.0 °C
62.5 %

@Temperature 73.4 °F
Modulus of Elasticity 207 GPa
30000 ksi
Compressive Yield Strength 365 MPa
52900 psi
Thermal Properties Metric English Comments
CTE, linear 16.6 µm/m-°C

@Temperature 20.0 - 100 °C
9.22 µin/in-°F

@Temperature 68.0 - 212 °F
18.0 µm/m-°C

@Temperature 20.0 - 316 °C
10.0 µin/in-°F

@Temperature 68.0 - 601 °F
18.0 µm/m-°C

@Temperature 20.0 - 358 °C
10.0 µin/in-°F

@Temperature 68.0 - 676 °F
20.3 µm/m-°C

@Temperature 20.0 - 871 °C
11.3 µin/in-°F

@Temperature 68.0 - 1600 °F
Specific Heat Capacity 0.502 J/g-°C

@Temperature 0.000 - 100 °C
0.120 BTU/lb-°F

@Temperature 32.0 - 212 °F
Thermal Conductivity 16.3 W/m-K

@Temperature 100 °C
113 BTU-in/hr-ft²-°F

@Temperature 212 °F
23.0 W/m-K

@Temperature 500 °C
160 BTU-in/hr-ft²-°F

@Temperature 932 °F
Melting Point 1400 - 1455 °C
2550 - 2651 °F
Solidus 1400 °C
2550 °F
Liquidus 1455 °C
2651 °F
Component Elements Properties Metric English Comments
Carbon, C <= 0.15 %
<= 0.15 %
Chromium, Cr 16 - 18 %
16 - 18 %
Iron, Fe 72 %
72 %
as balance
Manganese, Mn 5.5 - 7.5 %
5.5 - 7.5 %
Nickel, Ni 3.5 - 5.5 %
3.5 - 5.5 %
Nitrogen, N <= 0.25 %
<= 0.25 %
Silicon, Si <= 1.0 %
<= 1.0 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.0000670 ohm-cm
0.0000670 ohm-cm
Magnetic Permeability 1.004
1.004
D.C. Permeability (m at 200 H)
Users viewing this material also viewed the following: