Electrical Properties | Metric | English | Comments |
---|---|---|---|
Comparative Tracking Index | 400 - 499 V @Thickness 3.00 mm |
400 - 499 V @Thickness 0.118 in |
IEC 60112 |
Ascend Performance Materials Vydyne® R543H BK02 Nylon 66, 43% Glass Reinforced, DAM Vydyne® R543H BK02 is general-purpose, 43% glass-fiber reinforced PA66 resin. Available in black, it is an injection-molding grade resin that is lubricated for machine feed, flow and mold release. .. |
|||
Comparative Tracking Index | 400 - 499 V @Thickness 1.00 mm |
400 - 499 V @Thickness 0.0394 in |
IEC 60112 |
Ascend Performance Materials Vydyne® R550H Nylon 66, 50% Glass Reinforced, DAM Vydyne® R550H is general-purpose, heat-stabilized, hydrolysis-resistant, 50% glass-fiber reinforced PA66 resin. Available in natural, it is specifically designed to maximize the retention of physic.. |