| Category | Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK) |
| Manufacturer | Wolf Kunststoff |
| Trade Name | ZEDEX® |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Wolf Kunststoff ZEDEX® ZX-324V11T A3L PEEK Polymer, Reinforced.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 1.34 g/cc | 0.0484 lb/in³ | ISO 1183 |
| Water Absorption | 0.050 % @Temperature 23.0 °C |
0.050 % @Temperature 73.4 °F |
RMC 93%; DIN EN ISO 62 |
| Moisture Absorption at Equilibrium | 0.10 % | 0.10 % | DIN EN ISO 62 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore A | >= 100 | >= 100 | DIN 53505 |
| Hardness, Shore D | 85 | 85 | DIN 53505 |
| Ball Indentation Hardness | 190 MPa | 27600 psi | DIN 2039 |
| Tensile Strength at Break | 98.0 MPa | 14200 psi | DIN EN ISO 527 |
| Tensile Strength | 113 MPa | 16400 psi | DIN EN ISO 527 |
| Tensile Stress | 29.0 MPa @Strain 1.00 %, Time 3.60e+6 sec |
4210 psi @Strain 1.00 %, Time 1000 hour |
DIN 53444 |
| Tensile Strength, Yield | 78.0 MPa | 11300 psi | Elastic Limit |
| 113 MPa | 16400 psi | DIN EN ISO 527 | |
| Elongation at Break | 9.0 % | 9.0 % | |
| 9.0 % | 9.0 % | DIN EN ISO 527 | |
| Elongation at Yield | 1.3 % | 1.3 % | Elastic Yield Point |
| 5.0 % | 5.0 % | Elongation at Maximum Force; DIN EN ISO 527 | |
| 5.0 % | 5.0 % | DIN EN ISO 527 | |
| 6.6 % | 6.6 % | Flexural; DIN EN ISO 178 | |
| Tensile Modulus | 4.40 GPa | 638 ksi | DIN EN ISO 527 |
| Flexural Strength | 119 MPa | 17300 psi | Outer Fiber Stress at 3.5% Outer Fiber Strain; DIN EN ISO 178 |
| 159 MPa | 23100 psi | DIN EN ISO 178 | |
| Flexural Modulus | 2.937 GPa | 426.0 ksi | DIN EN ISO 178 |
| Compressive Yield Strength | 146 MPa | 21200 psi | DIN EN ISO 604 |
| Compressive Strength | 122 MPa | 17700 psi | Elastic Limit |
| 40.0 MPa @Time 3.60e+7 sec |
5800 psi @Time 10000 hour |
||
| 103 MPa @Time 360000 sec |
14900 psi @Time 100 hour |
||
| 130 MPa @Time 36.0 sec |
18900 psi @Time 0.0100 hour |
||
| 36.0 MPa @Strain 3.50 % |
5220 psi @Strain 3.50 % |
DIN EN ISO 604 | |
| Compressive Modulus | 2.85 GPa | 413 ksi | DIN EN ISO 604 |
| Fatigue Strength | 65.0 MPa @# of Cycles 1.00e+6 |
9430 psi @# of Cycles 1.00e+6 |
1 Hz |
| K Factor (ISO) | 1.2 µm/km @Temperature 200 °C |
1.2 µm/km @Temperature 392 °F |
|
| 3.7 µm/km @Temperature 240 °C |
3.7 µm/km @Temperature 464 °F |
||
| 9.1 µm/km @Temperature 100 °C |
9.1 µm/km @Temperature 212 °F |
||
| 12 µm/km @Temperature 20.0 °C |
12 µm/km @Temperature 68.0 °F |
||
| Charpy Impact Unnotched | NB | NB | EN ISO 179/1eU |
| Charpy Impact, Notched | 0.620 J/cm² | 2.95 ft-lb/in² | EN ISO 179/1eA |
| Coefficient of Friction, Dynamic | 0.14 @Temperature 20.0 °C |
0.14 @Temperature 68.0 °F |
Dry Operation |
| 0.21 @Temperature 100 °C |
0.21 @Temperature 212 °F |
Dry Operation | |
| Coefficient of Friction, Static | 0.18 @Temperature 20.0 °C |
0.18 @Temperature 68.0 °F |
Dry Operation |
| Tensile Creep Modulus, 1000 hours | 2780 MPa | 403000 psi | At 1% Deformation; DIN 53444 |
| Limiting Pressure Velocity | 0.300 MPa-m/sec | 8570 psi-ft/min | v = 200m/min |
| 0.33333 MPa-m/sec | 9516.6 psi-ft/min | v = 100m/min | |
| 0.91666 MPa-m/sec | 26171 psi-ft/min | v = 10m/min | |
| 1.00 MPa-m/sec | 28600 psi-ft/min | v = 1m/min | |
| Compression Set | 8.3 % | 8.3 % | Elastic Compression Limit |
| 12.5 % | 12.5 % | Nominal Compressive Yield Strain; DIN EN ISO 604 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 58.0 µm/m-°C @Temperature <=100 °C |
32.2 µin/in-°F @Temperature <=212 °F |
ISO E 830 |
| 58.0 µm/m-°C @Temperature <=150 °C |
32.2 µin/in-°F @Temperature <=302 °F |
ISO E 831 | |
| Specific Heat Capacity | 0.900 J/g-°C | 0.215 BTU/lb-°F | DSC |
| Thermal Conductivity | 0.240 W/m-K | 1.67 BTU-in/hr-ft²-°F | DIN 52612 |
| Melting Point | 340 °C | 644 °F | DSC |
| Maximum Service Temperature, Air | 140 °C | 284 °F | Pressed Bushings |
| 250 °C | 482 °F | Continuous | |
| 260 °C | 500 °F | Short Term (3h) | |
| Deflection Temperature at 1.8 MPa (264 psi) | 165 °C | 329 °F | DIN EN ISO 75 |
| Glass Transition Temp, Tg | 146 °C | 295 °F | DSC |
| Flammability, UL94 | V-0 | V-0 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | 4.00e+15 ohm-cm | 4.00e+15 ohm-cm | IEC 93 |
| Surface Resistance | 7.80e+11 ohm | 7.80e+11 ohm | IEC 93 |
| Dielectric Constant | 3.0 @Frequency 110 Hz |
3.0 @Frequency 110 Hz |
IEC 250 |
| Dielectric Strength | 26.0 kV/mm | 660 kV/in | IEC 243 |
| Dissipation Factor | 0.0020 | 0.0020 | IEC 112 |
| 0.053 @Frequency 1.00 Hz |
0.053 @Frequency 1.00 Hz |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Alignment Adjustment | 4 | Nominal Scale: 1, low; 10, high |
| Chemical Sterilization | 10 | Nominal Scale: 1, low; 10, high |
| Color | Black | |
| Creep Resistance | 5 | Nominal Scale: 1, low; 10, high |
| Dimensional Stability with Thermal Expansion | 5 | Nominal Scale: 1, low; 10, high |
| Free from Silicon | Applicable | |
| Gamma-rays Radiation Sterilization | 10 | Nominal Scale: 1, low; 10, high |
| High Precision Bushings (negative clearance) | Applicable | |
| Injection Molded Parts | Applicable | |
| Machined Parts | Applicable | |
| Moist Heat Sterilization | 10 | Nominal Scale: 1, low; 10, high |
| Plastic Granules | Applicable | |
| Resistance Against dust, Dirt, Abrasive Substances | 7 | Nominal Scale: 1, low; 10, high |
| Resistance Against Hot Water | 200 | |
| Resistance to Chemicals | 8 | Nominal Scale: 1, low; 10, high |
| Resistant Against Disinfectant | Applicable | |
| Rods up to Øe (de) | Applicable | |
| ROHS/WEEE | Applicable | |
| Sheets up to Maximum Thickness | Applicable | |
| Sliding Velocity | 100 | |
| Suitable for Outdoor Use | 7 | Nominal Scale: 1, low; 10, high |
| Suitable for Use in Water | Applicable | |
| Suitable for Vacuum | Applicable | |
| Tubes (hollow rods) up to Øe (de) | Applicable | |
| UV Rays Resistance | 9 | Nominal Scale: 1, low; 10, high |
| UV-Sterilization | 7 | Nominal Scale: 1, low; 10, high |