| Category | Ceramic , Glass |
| Manufacturer | Schott North America |
| Trade Name | |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Schott N-BAF51 Glass.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 3.33 g/cc | 0.120 lb/in³ |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Knoop Microhardness | 560 | 560 | .1/20 |
| Modulus of Elasticity | 91.0 GPa | 13200 ksi | |
| Poissons Ratio | 0.262 | 0.262 | |
| Shear Modulus | 36.0 GPa | 5220 ksi | calculated |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 8.40 µm/m-°C @Temperature -30.0 - 70.0 °C |
4.67 µin/in-°F @Temperature -22.0 - 158 °F |
|
| 9.50 µm/m-°C @Temperature 20.0 - 300 °C |
5.28 µin/in-°F @Temperature 68.0 - 572 °F |
||
| Specific Heat Capacity | 0.840 J/g-°C | 0.201 BTU/lb-°F | |
| Thermal Conductivity | 0.670 W/m-K | 4.65 BTU-in/hr-ft²-°F | |
| Transformation Temperature, Tg | 569 °C | 1060 °F |
| Optical Properties | Metric | English | Comments |
|---|---|---|---|
| Refractive Index | 1.65224 @Wavelength 587.6 nm |
1.65224 @Wavelength 587.6 nm |
n<sub>d</sub> |
| 1.65569 @Wavelength 546.1 nm |
1.65569 @Wavelength 546.1 nm |
n<sub>e</sub> | |
| Transmission, Visible | 86.2 % @Thickness 10.0 mm, Wavelength 380 nm |
86.2 % @Thickness 0.394 in, Wavelength 380 nm |
|
| 96.3 % @Thickness 10.0 mm, Wavelength 405 nm |
96.3 % @Thickness 0.394 in, Wavelength 405 nm |
||
| 98.8 % @Thickness 10.0 mm, Wavelength 460 nm |
98.8 % @Thickness 0.394 in, Wavelength 460 nm |
||
| 99.7 % @Thickness 10.0 mm, Wavelength 580 nm |
99.7 % @Thickness 0.394 in, Wavelength 580 nm |
||
| 99.7 % @Thickness 10.0 mm, Wavelength 700 nm |
99.7 % @Thickness 0.394 in, Wavelength 700 nm |
||
| IR Transmittance | 74.6 % @Thickness 10.0 mm, Wavelength 2500 nm |
74.6 % @Thickness 0.394 in, Wavelength 2500 nm |
|
| 99.2 % @Thickness 10.0 mm, Wavelength 1530 nm |
99.2 % @Thickness 0.394 in, Wavelength 1530 nm |
||
| UV Transmittance | 20.9 % @Thickness 10.0 mm, Wavelength 350 nm |
20.9 % @Thickness 0.394 in, Wavelength 350 nm |
|
| 64.2 % @Thickness 10.0 mm, Wavelength 365 nm |
64.2 % @Thickness 0.394 in, Wavelength 365 nm |
||
| 73.9 % @Thickness 10.0 mm, Wavelength 370 nm |
73.9 % @Thickness 0.394 in, Wavelength 370 nm |
| Chemical Properties | Metric | English | Comments |
|---|---|---|---|
| Acid Class, SR | 5.4 | 5.4 | |
| Alkali Class, AR | 1.3 | 1.3 | |
| Stain Resistance Class, FR | 0.00 | 0.00 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| B | 1 | |
| Climatic Resistance Test CR | 2 | |
| HG | 5 | |
| K (10-6mm2/N) | 2.22 | |
| Phosphate Resistance PR | 1 | |
| T1013.0 (°C) | 574 | |
| T107.6 (°C) | 712 |