Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Flexural Modulus | 0.138 - 1.77 GPa | 20.0 - 257 ksi | Average value: 0.736 GPa Grade Count:10 |
Overview of materials for Thermoplastic Olefinic Elastomer (TPO), Blow Molding Grade This property data is a summary of similar materials in the MatWeb database for the category "Thermoplastic Olefinic Elastomer (TPO), Blow Molding Grade". Each property range of values reported is m.. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | 2% Secant, 12.7 mm/min; ASTM D790 |
Eastman D4056-P Polyethylene
(discontinued **) Polyethylene D4056-P is a natural low density material with an 80 melt index.Eastman Chemical Company sold its polyethylene business to Westlake Chemical Corporation in Dec. 2006. This grade no lon.. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
Multibase Multi-Flex® D 4201 TPE Thermoplastic Elastomer Features: Chemical Resistance, Good Heat StabilizedOzone Resistant General Purpose Forms:PelletsProcessing Method:Injection MoldingBlow MoldingExtrusion Uses: Automotive ApplicationsInformation p.. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
Multibase Multi-Flex® G 7827 Black TPE Styrene Ethylene Butylene Styrene Block Copolymer Forms: PelletsProcessing Methods:Injection Molding Uses: Automotive ApplicationsInformation provided by Multibase |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
A. Schulman POLYTROPE™ TPP 402 Blow Molding Grade Olefinic Thermoplastic Elastomer DescriptionPolytrope TPP 402 is a blow molding grade olefinic thermoplastic elastomer. This elastomer is specifically designed for flexible, automotive under-hood air ducts. This product contains .. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
Teknor Apex TEKRON® 4300-D88A Thermoplastic Elastomer Information provided by Teknor Apex Company |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
Teknor Apex TEKRON® 4300LM-P88-1 Thermoplastic Elastomer Information provided by Teknor Apex Company |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
Teknor Apex Telcar® TL EF-6100 Thermoplastic Elastomer Uses: Automotive Applications; Automotive Exterior Parts; Automotive Exterior Trim; Automotive Interior Parts; Blow Molding Applications; General Purpose; Grommets; Weatherstripping Forms: Pellets P.. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
DuPont Keldax® 6868 Filled Thermoplastic Ethylene Polymer A low fog filled thermoplastic ethylene polymer that provides acoustical sound barrier performance in automotive, construction, and industrial applications.Processing Method: ExtrusionSheetAvailabil.. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
A. Schulman POLYTROPE™ TPP 402 Blow Molding Grade Olefinic Thermoplastic Elastomer DescriptionPolytrope TPP 402 is a blow molding grade olefinic thermoplastic elastomer. This elastomer is specifically designed for flexible, automotive under-hood air ducts. This product contains .. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
A. Schulman POLYTROPE™ TPP 402 Blow Molding Grade Olefinic Thermoplastic Elastomer DescriptionPolytrope TPP 402 is a blow molding grade olefinic thermoplastic elastomer. This elastomer is specifically designed for flexible, automotive under-hood air ducts. This product contains .. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
A. Schulman POLYTROPE™ TPP 402 Blow Molding Grade Olefinic Thermoplastic Elastomer DescriptionPolytrope TPP 402 is a blow molding grade olefinic thermoplastic elastomer. This elastomer is specifically designed for flexible, automotive under-hood air ducts. This product contains .. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
A. Schulman POLYTROPE™ TPP 402 Blow Molding Grade Olefinic Thermoplastic Elastomer DescriptionPolytrope TPP 402 is a blow molding grade olefinic thermoplastic elastomer. This elastomer is specifically designed for flexible, automotive under-hood air ducts. This product contains .. |
|||
Flexural Modulus | 0.138 GPa | 20.0 ksi | ASTM D790 |
A. Schulman POLYTROPE™ TPP 402 Blow Molding Grade Olefinic Thermoplastic Elastomer DescriptionPolytrope TPP 402 is a blow molding grade olefinic thermoplastic elastomer. This elastomer is specifically designed for flexible, automotive under-hood air ducts. This product contains .. |