Category Polymer , Thermoplastic , Fluoropolymer , PFA , Polyperfluoroalkoxyethylene, Molded/Extruded
Manufacturer Zeus
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Zeus PFA Tubing.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
PFA, or perfluoroalkoxy, is well recognized for its ability to maintain mechanical integrity in extreme temperatures even when exposed to caustic chemicals. PFA comes in high purity versions that are SEMI F-57 certified, lending itself to critical fluid transport tubing applications that demand a very low level of extractables. This fluoropolymer can be extruded in convoluted tubing forms that provide a highly flexible conduit.
Physical Properties Metric English Comments
Density 2.12 - 2.17 g/cc
0.0766 - 0.0784 lb/in³
ASTM D792
Water Absorption <= 0.030 %
<= 0.030 %
ASTM D257
Crystallinity 48 - 70 %
48 - 70 %
Mechanical Properties Metric English Comments
Hardness, Shore D 55 - 60
55 - 60
ASTM D2240
Tensile Strength, Ultimate 25.0 - 35.0 MPa
3630 - 5080 psi
ASTM D638
Elongation at Break 250 - 420 %
250 - 420 %
ASTM D638
Modulus of Elasticity 0.450 GPa
65.3 ksi
ASTM D638
Flexural Modulus 0.600 - 0.700 GPa
87.0 - 102 ksi
ASTM D790
Coefficient of Friction 0.040 - 0.20
0.040 - 0.20
Thermal Properties Metric English Comments
CTE, linear 120 - 140 µm/m-°C

@Temperature 20.0 °C
66.7 - 77.8 µin/in-°F

@Temperature 68.0 °F
ASTM D696
Thermal Conductivity 0.150 - 0.250 W/m-K
1.04 - 1.74 BTU-in/hr-ft²-°F
ASTM C177
Melting Point 300 - 315 °C
572 - 599 °F
Maximum Service Temperature, Air 260 °C
500 °F
Minimum Service Temperature, Air -200 °C
-328 °F
Glass Transition Temp, Tg 100 °C
212 °F
Decomposition Temperature 475 °C
887 °F
ASTM E1131
Oxygen Index >= 95 %
>= 95 %
ASTM D2863
Optical Properties Metric English Comments
Refractive Index 1.35
1.35
Electrical Properties Metric English Comments
Volume Resistivity 1.00e+18 ohm-cm
1.00e+18 ohm-cm
ASTM D257
Dielectric Constant 1.9 - 2.1

@Frequency 1.00e+6 Hz
1.9 - 2.1

@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 19.7 - 78.7 kV/mm
500 - 2000 kV/in
ASTM D149
Descriptive Properties Value Comments
Radiation Resistance (MRad) 1 to 10