Wolf Kunststoff ZEDEX® ZX-324V1T A3H PEEK Polymer, Reinforced

Category Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK)
Manufacturer Wolf Kunststoff
Trade Name ZEDEX®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Wolf Kunststoff ZEDEX® ZX-324V1T A3H PEEK Polymer, Reinforced.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Main Characteristics: High resilience; High elasticity; Low permanent deformation; Stress resistant; High strength at temperatures above 140 ° CApplications: Shipbuilding; Chemical Engineering; Automitve Technology; Machine ToolsInformation provided by Zedex
Physical Properties Metric English Comments
Density 1.33 g/cc
0.0480 lb/in³
ISO 1183
Water Absorption 0.10 %

@Temperature 23.0 °C
0.10 %

@Temperature 73.4 °F
RMC 93%; DIN EN ISO 62
Moisture Absorption at Equilibrium 0.50 %
0.50 %
DIN EN ISO 62
Mechanical Properties Metric English Comments
Hardness, Shore A >= 100
>= 100
DIN 53505
Hardness, Shore D 86
86
DIN 53505
Ball Indentation Hardness 175 MPa
25400 psi
DIN 2039
Tensile Strength at Break 117 MPa
17000 psi
DIN EN ISO 527
Tensile Strength 117 MPa
17000 psi
DIN EN ISO 527
Tensile Stress 32.0 MPa

@Strain 1.00 %,
Time 3.60e+6 sec
4640 psi

@Strain 1.00 %,
Time 1000 hour
DIN 53444
Tensile Strength, Yield 74.0 MPa
10700 psi
Elastic Limit
Elongation at Break 10.1 %
10.1 %
10.1 %
10.1 %
DIN EN ISO 527
Elongation at Yield 5.0 %
5.0 %
Elastic Yield Point
6.2 %
6.2 %
Flexural; DIN EN ISO 178
10.1 %
10.1 %
Elongation at Maximum Force; DIN EN ISO 527
Tensile Modulus 3.50 GPa
508 ksi
DIN EN ISO 527
Flexural Strength 117.5 MPa
17040 psi
Outer Fiber Stress at 3.5% Outer Fiber Strain; DIN EN ISO 178
143 MPa
20700 psi
DIN EN ISO 178
Flexural Modulus 3.90 GPa
566 ksi
DIN EN ISO 178
Compressive Yield Strength 145 MPa
21000 psi
DIN EN ISO 604
Compressive Strength 119 MPa
17300 psi
Elastic Limit
43.0 MPa

@Time 3.60e+7 sec
6240 psi

@Time 10000 hour
102 MPa

@Time 360000 sec
14800 psi

@Time 100 hour
127 MPa

@Time 36.0 sec
18400 psi

@Time 0.0100 hour
145 MPa

@Strain 3.50 %
21000 psi

@Strain 3.50 %
DIN EN ISO 604
Compressive Modulus 3.70 GPa
537 ksi
DIN EN ISO 604
Fatigue Strength 70.0 MPa

@# of Cycles 1.00e+6
10200 psi

@# of Cycles 1.00e+6
1 Hz
K Factor (ISO) 1.0 µm/km

@Temperature 200 °C
1.0 µm/km

@Temperature 392 °F
1.4 µm/km

@Temperature 100 °C
1.4 µm/km

@Temperature 212 °F
2.4 µm/km

@Temperature 240 °C
2.4 µm/km

@Temperature 464 °F
3.4 µm/km

@Temperature 20.0 °C
3.4 µm/km

@Temperature 68.0 °F
Charpy Impact Unnotched NB
NB
EN ISO 179/1eU
Charpy Impact, Notched 0.630 J/cm²
3.00 ft-lb/in²
EN ISO 179/1eA
Coefficient of Friction, Dynamic 0.13

@Temperature 20.0 °C
0.13

@Temperature 68.0 °F
Dry Operation
0.20

@Temperature 100 °C
0.20

@Temperature 212 °F
Dry Operation
Coefficient of Friction, Static 0.11

@Temperature 20.0 °C
0.11

@Temperature 68.0 °F
Dry Operation
Tensile Creep Modulus, 1000 hours 3040 MPa
441000 psi
At 1% Deformation; DIN 53444
Limiting Pressure Velocity 0.350 MPa-m/sec
9990 psi-ft/min
v = 10m/min
0.400 MPa-m/sec
11400 psi-ft/min
v = 100m/min
0.400 MPa-m/sec
11400 psi-ft/min
v = 200m/min
0.8455 MPa-m/sec
24140 psi-ft/min
v = 1m/min
Compression Set 1.7 %
1.7 %
Elastic Compression Limit
2.5 %
2.5 %
Nominal Compressive Yield Strain; DIN EN ISO 604
Thermal Properties Metric English Comments
CTE, linear 47.0 µm/m-°C

@Temperature <=100 °C
26.1 µin/in-°F

@Temperature <=212 °F
ISO E 830
59.0 µm/m-°C

@Temperature <=150 °C
32.8 µin/in-°F

@Temperature <=302 °F
ISO E 831
Specific Heat Capacity 1.09 J/g-°C
0.261 BTU/lb-°F
DSC
Melting Point 340 °C
644 °F
DSC
Maximum Service Temperature, Air 140 °C
284 °F
Pressed Bushings
250 °C
482 °F
Continuous
260 °C
500 °F
Short Term (3h)
Deflection Temperature at 1.8 MPa (264 psi) 170 °C
338 °F
DIN EN ISO 75
Glass Transition Temp, Tg 170 °C
338 °F
DSC
Flammability, UL94 V-0
V-0
Oxygen Index 16 %
16 %
DIN EN ISO 4589
Electrical Properties Metric English Comments
Volume Resistivity 5.00e+16 ohm-cm
5.00e+16 ohm-cm
IEC 93
Surface Resistance 3.20e+12 ohm
3.20e+12 ohm
IEC 93
Dielectric Constant 3.1

@Frequency 110 Hz
3.1

@Frequency 110 Hz
IEC 250
Dielectric Strength 25.0 kV/mm
635 kV/in
IEC 243
Dissipation Factor 0.0020
0.0020
IEC 112
0.061

@Frequency 1.00 Hz
0.061

@Frequency 1.00 Hz
Descriptive Properties Value Comments
Alignment Adjustment 4
Nominal Scale: 1, low; 10, high
Chemical Sterilization 7
Nominal Scale: 1, low; 10, high
Color Beige
Creep Resistance 5
Nominal Scale: 1, low; 10, high
Dimensional Stability with Thermal Expansion 5
Nominal Scale: 1, low; 10, high
Free from Silicon Applicable
Gamma-rays Radiation Sterilization 10
Nominal Scale: 1, low; 10, high
High Precision Bushings (negative clearance) Applicable
Injection Molded Parts Applicable
Machined Parts Applicable
Moist Heat Sterilization 10
Nominal Scale: 1, low; 10, high
Plastic Granules Applicable
Resistance Against dust, Dirt, Abrasive Substances 7
Nominal Scale: 1, low; 10, high
Resistance Against Hot Water 140
Resistance to Chemicals 7
Nominal Scale: 1, low; 10, high
Resistant Against Disinfectant Applicable
Rods up to Øe (de) Applicable
Sheets up to Maximum Thickness Applicable
Sliding Velocity 100
Suitable for Outdoor Use 7
Nominal Scale: 1, low; 10, high
Suitable for Use in Water Applicable
Suitable for Vacuum Applicable
Tubes (hollow rods) up to Øe (de) Applicable
UV Rays Resistance 9
Nominal Scale: 1, low; 10, high
UV-Sterilization 7
Nominal Scale: 1, low; 10, high