Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Solvay Specialty Polymers Udel® P-1750 MR Polysulfone (PSU)  (Unverified Data**)

Category Polymer , Thermoplastic , Polysulfone (PSU)
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Solvay Specialty Polymers Udel® P-1750 MR Polysulfone (PSU)  (Unverified Data**).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Udel P-1750 MR is a lower color grade of polysulfone that contains a mold release which aids part ejection when parts with low draft are injection molded. Polysulfones have long been known for transparency and clarity, but have been somewhat limited by a slight yellow cast which has been typical of the material. These grades were designed to eliminate the yellow cast and provide improved aesthetics for applications where a yellow cast is undesirable. In general, Udel polysulfone is a tough, rigid, high-strength, high-heat thermoplastic that retains its properties at temperatures from -101°C to 149°C (-150°F to 300°F). With a heat deflection temperature at 1.8 MPa (264 psi) of 174°C (345°F) and excellent thermal and oxidative stability, this resin is suitable for sustained use at temperatures up to 149°C (300°F). Other key properties of polysulfone include resistance to hydrolysis by hot water and resistance to acids and bases. In addition, the resin is resistant to a wide range of cleaners and disinfectants. Polysulfone's resistance to alcohols and aliphatic hydrocarbons is also good; however, the resin is generally not resistant to polar organic or chlorinated solvents. - Natural/Transparent: Udel P-1750 NT MRInformation provided by Solvay Specialty Polymers.
Physical Properties Metric English Comments
Specific Gravity 1.24 g/cc
1.24 g/cc
ASTM D792
Water Absorption 0.30 %

@Time 86400 sec
0.30 %

@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0070 cm/cm
0.0070 in/in
ASTM D955
Melt Flow 6.5 g/10 min

@Load 2.06 kg,
Temperature 343 °C
6.5 g/10 min

@Load 4.54 lb,
Temperature 649 °F
ASTM D1238
Mechanical Properties Metric English Comments
Tensile Strength 70.3 MPa
10200 psi
ASTM D638
Elongation at Break 50 - 100 %
50 - 100 %
ASTM D638
Tensile Modulus 2.48 GPa
360 ksi
ASTM D638
Flexural Strength 106 MPa
15400 psi
ASTM D790
Flexural Modulus 2.69 GPa
390 ksi
ASTM D790
Izod Impact, Notched 0.690 J/cm
1.29 ft-lb/in
ASTM D256
Tensile Impact Strength 420 kJ/m²
200 ft-lb/in²
ASTM D1822
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 56.0 µm/m-°C
31.1 µin/in-°F
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 174 °C
345 °F
Unannealed; ASTM D648
Electrical Properties Metric English Comments
Volume Resistivity 3.00e+16 ohm-cm
3.00e+16 ohm-cm
ASTM D257
Dielectric Constant 2.9

@Frequency 60.0 Hz
2.9

@Frequency 60.0 Hz
ASTM D150
3.02

@Frequency 1.00e+6 Hz
3.02

@Frequency 1.00e+6 Hz
ASTM D150
3.04

@Frequency 1000 Hz
3.04

@Frequency 1000 Hz
ASTM D150
Dielectric Strength 17.0 kV/mm
432 kV/in
ASTM D149
Dissipation Factor 0.00070

@Frequency 60.0 Hz
0.00070

@Frequency 60.0 Hz
ASTM D150
0.0010

@Frequency 1000 Hz
0.0010

@Frequency 1000 Hz
ASTM D150
0.0060

@Frequency 1.00e+6 Hz
0.0060

@Frequency 1.00e+6 Hz
ASTM D150
Processing Properties Metric English Comments
Melt Temperature 329 - 385 °C
624 - 725 °F
Mold Temperature 121 - 163 °C
250 - 325 °F
Drying Temperature 135 - 163 °C
275 - 325 °F
Dry Time 3.50 hour
3.50 hour
Shot Size 50 - 75 %
50 - 75 %
Descriptive Properties Value Comments
Appearance Clear/Transparent
Availability Asia Pacific
Europe
North America
South America
Features Acid Resistant
Alcohol Resistant
Alkali Resistant
Good Chemical Resistance
Good Toughness
High Heat Resistance
Hydrocarbon Resistant
Hydrolytically Stable
Forms Pellets
Generic PSU
Processing Method Extrusion
Injection Molding
Uses Appliance Components
Appliances
Automotive Electronics
Batteries
Business Equipment
Electrical Parts
Electrical/Electronic Applications
Food Service Applications
Industrial Parts
Microwave Cookware
Piping
Plumbing Parts
Valves/Valve Parts
Copyright © lookpolymers.com All Rights Reserved