Schott N-LAK10 Glass

Category Ceramic , Glass
Manufacturer Schott North America
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Schott N-LAK10 Glass.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Information Provided by SCHOTT North America, Inc.
Physical Properties Metric English Comments
Density 3.69 g/cc
0.133 lb/in³
Mechanical Properties Metric English Comments
Knoop Microhardness 780
780
.1/20
Modulus of Elasticity 116 GPa
16800 ksi
Poissons Ratio 0.286
0.286
Shear Modulus 45.0 GPa
6530 ksi
calculated
Thermal Properties Metric English Comments
CTE, linear 5.70 µm/m-°C

@Temperature -30.0 - 70.0 °C
3.17 µin/in-°F

@Temperature -22.0 - 158 °F
6.80 µm/m-°C

@Temperature 20.0 - 300 °C
3.78 µin/in-°F

@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.640 J/g-°C
0.153 BTU/lb-°F
Thermal Conductivity 0.860 W/m-K
5.97 BTU-in/hr-ft²-°F
Transformation Temperature, Tg 636 °C
1180 °F
Optical Properties Metric English Comments
Refractive Index 1.72003

@Wavelength 587.6 nm
1.72003

@Wavelength 587.6 nm
n<sub>d</sub>
1.72341

@Wavelength 546.1 nm
1.72341

@Wavelength 546.1 nm
n<sub>e</sub>
Transmission, Visible 90.1 %

@Thickness 10.0 mm,
Wavelength 380 nm
90.1 %

@Thickness 0.394 in,
Wavelength 380 nm
96.3 %

@Thickness 10.0 mm,
Wavelength 405 nm
96.3 %

@Thickness 0.394 in,
Wavelength 405 nm
99.1 %

@Thickness 10.0 mm,
Wavelength 460 nm
99.1 %

@Thickness 0.394 in,
Wavelength 460 nm
99.7 %

@Thickness 10.0 mm,
Wavelength 580 nm
99.7 %

@Thickness 0.394 in,
Wavelength 580 nm
99.9 %

@Thickness 10.0 mm,
Wavelength 700 nm
99.9 %

@Thickness 0.394 in,
Wavelength 700 nm
IR Transmittance 42.8 %

@Thickness 10.0 mm,
Wavelength 2500 nm
42.8 %

@Thickness 0.394 in,
Wavelength 2500 nm
99.1 %

@Thickness 10.0 mm,
Wavelength 1530 nm
99.1 %

@Thickness 0.394 in,
Wavelength 1530 nm
UV Transmittance 2.6 %

@Thickness 10.0 mm,
Wavelength 334 nm
2.6 %

@Thickness 0.394 in,
Wavelength 334 nm
44.2 %

@Thickness 10.0 mm,
Wavelength 350 nm
44.2 %

@Thickness 0.394 in,
Wavelength 350 nm
77 %

@Thickness 10.0 mm,
Wavelength 365 nm
77 %

@Thickness 0.394 in,
Wavelength 365 nm
83.1 %

@Thickness 10.0 mm,
Wavelength 370 nm
83.1 %

@Thickness 0.394 in,
Wavelength 370 nm
Chemical Properties Metric English Comments
Acid Class, SR 52.3
52.3
Alkali Class, AR 1.0
1.0
Stain Resistance Class, FR 2.0
2.0
Descriptive Properties Value Comments
B 0
Climatic Resistance Test CR 2
HG 2
K (10-6mm2/N) 1.97
Phosphate Resistance PR 3
T1013.0 (°C) 631
T107.6 (°C) 714