Material Notes:
Transparent, enhanced flow Polyetherimide (Tg 217C) with internal mold release. ECO Conforming, U.S. FDA and EU Food Contact compliant.
Physical Properties Metric English Comments
Specific Gravity 1.27 g/cc
1.27 g/cc
ASTM D792
Density 1.27 g/cc
0.0459 lb/in³
ISO 1183
Water Absorption 0.25 %

@Time 86400 sec
0.25 %

@Time 24.0 hour
ASTM D570
Moisture Absorption 0.700 %
0.700 %
23°C / 50% RH; ISO 62
Moisture Absorption at Equilibrium 1.25 %
1.25 %
ASTM D570
Water Absorption at Saturation 1.25 %
1.25 %
ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
0.0050 - 0.0070 in/in
on Tensile Bar; SABIC Method
0.0050 - 0.0070 cm/cm

@Thickness 3.20 mm
0.0050 - 0.0070 in/in

@Thickness 0.126 in
SABIC Method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm

@Thickness 3.20 mm
0.0050 - 0.0070 in/in

@Thickness 0.126 in
SABIC Method
Melt Flow 12 g/10 min

@Load 6.60 kg,
Temperature 337 °C
12 g/10 min

@Load 14.6 lb,
Temperature 639 °F
ASTM D1238
Melt Index of Compound 17 g/10 min

@Load 5.00 kg,
Temperature 360 °C
17 g/10 min

@Load 11.0 lb,
Temperature 680 °F
MVR [cm^3/10 min]; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 85.0 MPa
12300 psi
Type I, 5 mm/min; ASTM D638
85.0 MPa
12300 psi
5 mm/min; ISO 527
Tensile Strength, Yield 105 MPa
15200 psi
5 mm/min; ISO 527
110 MPa
16000 psi
Type I, 5 mm/min; ASTM D638
Elongation at Break 60 %
60 %
Type I, 5 mm/min; ASTM D638
60 %
60 %
5 mm/min; ISO 527
Elongation at Yield 6.0 %
6.0 %
5 mm/min; ISO 527
7.0 %
7.0 %
Type I, 5 mm/min; ASTM D638
Tensile Modulus 3.20 GPa
464 ksi
1 mm/min; ISO 527
3.59 GPa
521 ksi
5 mm/min; ASTM D638
Flexural Yield Strength 160 MPa
23200 psi
2 mm/min; ISO 178
165 MPa
23900 psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.30 GPa
479 ksi
2 mm/min; ISO 178
3.52 GPa
511 ksi
1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 0.530 J/cm
0.993 ft-lb/in
ASTM D256
13.35 J/cm

@Thickness 3.20 mm
25.01 ft-lb/in

@Thickness 0.126 in
ASTM D256
Izod Impact, Unnotched 13.35 J/cm
25.01 ft-lb/in
ASTM D4812
Izod Impact, Notched (ISO) 6.00 kJ/m²
2.86 ft-lb/in²
80*10*4; ISO 180/1A
6.00 kJ/m²

@Temperature -30.0 °C
2.86 ft-lb/in²

@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NB
NB
80*10*4; ISO 180/1U
NB

@Temperature -30.0 °C
NB

@Temperature -22.0 °F
80*10*4; ISO 180/1U
Charpy Impact Unnotched NB
NB
Edgew 80*10*4 sp=62mm; ISO 179/1eU
NB

@Temperature -30.0 °C
NB

@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 0.400 J/cm²
1.90 ft-lb/in²
Edgew 80*10*4 sp=62mm; ISO 179/1eA
0.400 J/cm²

@Temperature -30.0 °C
1.90 ft-lb/in²

@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 38.0 J

@Temperature 23.0 °C
28.0 ft-lb

@Temperature 73.4 °F
ASTM D3763
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 55.0 µm/m-°C

@Temperature -40.0 - 150 °C
30.6 µin/in-°F

@Temperature -40.0 - 302 °F
ASTM E 831
55.0 µm/m-°C

@Temperature 23.0 - 150 °C
30.6 µin/in-°F

@Temperature 73.4 - 302 °F
ISO 11359-2
CTE, linear, Transverse to Flow 55.0 µm/m-°C

@Temperature -40.0 - 150 °C
30.6 µin/in-°F

@Temperature -40.0 - 302 °F
ASTM E 831
55.0 µm/m-°C

@Temperature 23.0 - 150 °C
30.6 µin/in-°F

@Temperature 73.4 - 302 °F
ISO 11359-2
Thermal Conductivity 0.220 W/m-K
1.53 BTU-in/hr-ft²-°F
ASTM C177
0.240 W/m-K
1.67 BTU-in/hr-ft²-°F
ISO 8302
Deflection Temperature at 0.46 MPa (66 psi) 198 °C
388 °F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
200 °C
392 °F
Edgew 120*10*4 sp=100mm; ISO 75/Be
207 °C

@Thickness 3.20 mm
405 °F

@Thickness 0.126 in
unannealed; ASTM D648
210 °C

@Thickness 6.40 mm
410 °F

@Thickness 0.252 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 188 °C
370 °F
Flatw 80*10*4 sp=64mm; ISO 75/Af
190 °C
374 °F
Edgew 120*10*4 sp=100mm; ISO 75/Ae
199 °C

@Thickness 3.20 mm
390 °F

@Thickness 0.126 in
unannealed; ASTM D648
201 °C

@Thickness 6.40 mm
394 °F

@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point 211 °C
412 °F
Rate B/50; ISO 306
212 °C
414 °F
Rate B/120; ISO 306
215 °C
419 °F
Rate A/50; ISO 306
219 °C
426 °F
Rate B/50; ASTM D1525
Glass Transition Temp, Tg 217 °C
423 °F
Optical Properties Metric English Comments
Transmission, Visible 90 %
90 %
transparent; thickness not quantified
Descriptive Properties Value Comments
Ball Pressure Test, 125°C +/- 2°C Passes
IEC 60695-10-2