Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

SABIC Innovative Plastics LNP VERTON RX06097 PA 66 (Europe-Africa-Middle East)

Category Polymer , Thermoplastic , Nylon , Nylon 66
Manufacturer SABIC Innovative Plastics (GE Plastics)
Trade Name LNP VERTON
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF SABIC Innovative Plastics LNP VERTON RX06097 PA 66 (Europe-Africa-Middle East).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
LNP* VERTON* RX06097 is a compound based on PA 66 resin containing Long Glass Fiber. Added features include; Easy Molding, UV-Stabilized.
Physical Properties Metric English Comments
Density 1.59 g/cc
0.0574 lb/in³
ISO 1183
Water Absorption 1.0 %

@Time 86400 sec
1.0 %

@Time 24.0 hour
ISO 62-1
Linear Mold Shrinkage, Flow 0.0032 cm/cm

@Time 86400 sec
0.0032 in/in

@Time 24.0 hour
ISO 294
Linear Mold Shrinkage, Transverse 0.0076 cm/cm

@Time 86400 sec
0.0076 in/in

@Time 24.0 hour
ISO 294
Mechanical Properties Metric English Comments
Tensile Strength at Break 275 MPa
39900 psi
5 mm/min; ISO 527
Elongation at Break 1.9 %
1.9 %
5 mm/min; ISO 527
2.8 %
2.8 %
Flexural Strain, break, 2 mm/min; ISO 178
Tensile Modulus 17.6 GPa
2550 ksi
1 mm/min; ISO 527
Flexural Strength 366 MPa
53100 psi
2 mm/min; ISO 178
Flexural Modulus 15.0 GPa
2180 ksi
2 mm/min; ISO 178
Izod Impact, Notched (ISO) 45.0 kJ/m²
21.4 ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 90.0 kJ/m²
42.8 ft-lb/in²
80*10*4; ISO 180/1U
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 260 °C
500 °F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi) 257 °C
495 °F
Flatw 80*10*4 sp=64mm; ISO 75/Af
Copyright © lookpolymers.com All Rights Reserved