Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Renegade Materials Corporation RM-3002 Bismaleimide (BMI) Resin T650-35-6K-UC309-5HS Carbon Fabric

Category Polymer , Thermoset , Filled/Reinforced Thermoset
Manufacturer Renegade Materials Corporation
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Renegade Materials Corporation RM-3002 Bismaleimide (BMI) Resin T650-35-6K-UC309-5HS Carbon Fabric.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Developed using state-of-the-art formulating technologies, RM-3002 BMI prepreg products deliver superior hot/wet performance in airframe, missile and propulsion applications at service temperatures up to 400°F. RM-3002 “next-generation” BMI delivers improved damage tolerance at higher temperatures vs. industry-standard BMI’s. Renegade precision-quality prepregs exhibit excellent handling characteristics and are available in woven and unidirectional form on various fibers including carbon, quartz and S2 glass. A wide variety of nano-materials can be incorporated into this resin system for tailored laminate properties and multi-functional performance. Renegade offers paste (RM-3006 and RM-3007) and film (RM-3011) adhesives compatible with RM-3002. Renegade also offers similar resin systems for RTM (RM-3000) or VARTM (RM-3010) processing.Information provided by Renegade Materials Corporation. Typical properties. Tensile and flexural data has been normalized to 60% fiber volume.
Physical Properties Metric English Comments
Density 1.26 g/cc
0.0456 lb/in³
Resin
Mechanical Properties Metric English Comments
Tensile Strength 889 MPa
129000 psi
Dry, RT, 0° Direction; ASTM D3039
1010 MPa
146000 psi
Dry, RT, 90° Direction; ASTM D3039
Elongation at Break 3.6 %
3.6 %
Resin
Tensile Modulus 75.2 GPa
10900 ksi
Dry, RT, 0° Direction; ASTM D3039
75.2 GPa
10900 ksi
Dry, RT, 90° Direction; ASTM D3039
Flexural Strength 145 MPa
21000 psi
Resin
951 MPa

@Temperature 204 °C
138000 psi

@Temperature 400 °F
Dry, 90° Direction; ASTM D790
1030 MPa

@Temperature 177 °C
150000 psi

@Temperature 350 °F
Dry, 90° Direction; ASTM D790
1080 MPa

@Temperature 21.1 °C
157000 psi

@Temperature 70.0 °F
Dry, 0° Direction; ASTM D790
1120 MPa

@Temperature 21.1 °C
163000 psi

@Temperature 70.0 °F
Dry, 90° Direction; ASTM D790
Flexural Modulus 4.27 GPa
620 ksi
Resin
61.4 GPa

@Temperature 21.1 °C
8900 ksi

@Temperature 70.0 °F
Dry, 90° Direction; ASTM D790
61.4 GPa

@Temperature 177 °C
8900 ksi

@Temperature 350 °F
Dry, 90° Direction; ASTM D790
63.4 GPa

@Temperature 204 °C
9200 ksi

@Temperature 400 °F
Dry, 90° Direction; ASTM D790
71.0 GPa

@Temperature 21.1 °C
10300 ksi

@Temperature 70.0 °F
Dry, 0° Direction; ASTM D790
Compressive Strength 592 MPa

@Temperature 204 °C
85800 psi

@Temperature 400 °F
Dry, 90° Direction; ASTM D695
781.9 MPa

@Temperature 21.1 °C
113400 psi

@Temperature 70.0 °F
Dry, 90° Direction; ASTM D695
786 MPa

@Temperature 21.1 °C
114000 psi

@Temperature 70.0 °F
Dry, 0° Direction; ASTM D695
Compressive Modulus 64.1 GPa

@Temperature 21.1 °C
9300 ksi

@Temperature 70.0 °F
Dry, 90° Direction; ASTM D695
68.3 GPa

@Temperature 21.1 °C
9900 ksi

@Temperature 70.0 °F
Dry, 0° Direction; ASTM D695
70.3 GPa

@Temperature 204 °C
10200 ksi

@Temperature 400 °F
Dry, 90° Direction; ASTM D695
Shear Strength 76.5 MPa
11100 psi
Short Beam, Dry, RT, 90° Direction; ASTM D2344
80.7 MPa
11700 psi
Short Beam, Dry, RT, 0° Direction; ASTM D2344
Copyright © lookpolymers.com All Rights Reserved