RTP Company RTP 699 X 94678 SSC-63386 Acrylonitrile Butadiene Styrene (ABS), Phosphorescent Green

Category Polymer , Thermoplastic , ABS Polymer
Manufacturer RTP Company
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF RTP Company RTP 699 X 94678 SSC-63386 Acrylonitrile Butadiene Styrene (ABS), Phosphorescent Green.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This material passes Mitsubishi and Toyota Glow Material Specifications for trunk latch release levers.
Physical Properties Metric English Comments
Specific Gravity 1.17 g/cc
1.17 g/cc
ASTM D 792
Linear Mold Shrinkage 0.0030 - 0.0080 cm/cm

@Thickness 3.17 mm
0.0030 - 0.0080 in/in

@Thickness 0.125 in
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength at Break 39.3 MPa
5700 psi
ASTM D 638
Elongation at Break 10 %
10 %
ASTM D 638
Tensile Modulus 2.07 GPa
300 ksi
ASTM D 638
Flexural Strength 72.4 MPa
10500 psi
ASTM D 790
Flexural Modulus 2.28 GPa
330 ksi
ASTM D 790
Izod Impact, Notched 0.694 J/cm

@Thickness 3.17 mm
1.30 ft-lb/in

@Thickness 0.125 in
D 256
Izod Impact, Unnotched 3.20 J/cm

@Thickness 3.17 mm
6.00 ft-lb/in

@Thickness 0.125 in
ASTM D4812
Processing Properties Metric English Comments
Melt Temperature 204 - 238 °C
400 - 460 °F
Mold Temperature 62.8 - 85.0 °C
145 - 185 °F
Drying Temperature 82.2 °C
180 °F
Dry Time 2 hour
2 hour
Moisture Content 0.10 %
0.10 %
Dew Point -17.8 °C
0.000 °F
Injection Pressure 68.9 - 103 MPa
10000 - 15000 psi